ARTICLE
Received 29 Nov 2013 | Accepted 3 Jul 2014 | Published 7 Aug 2014
Claudia Backes1,2, Ronan J. Smith1,2, Niall McEvoy1,3, Nina C. Berner1,3, David McCloskey1,2, Hannah C. Nerl1,2,3, Arlene ONeill1,2, Paul J. King1,2, Tom Higgins1,2, Damien Hanlon1,2, Nils Scheuschner4, Janina Maultzsch4, Lothar Houben5, Georg S. Duesberg1,3, John F. Donegan1,2, Valeria Nicolosi1,2,3 & Jonathan N. Coleman1,2
Two-dimensional nanomaterials such as MoS2 are of great interest both because of their novel physical properties and their applications potential. Liquid exfoliation, an important production method, is limited by our inability to quickly and easily measure nanosheet size, thickness or concentration. Here we demonstrate a method to simultaneously determine mean values of these properties from an optical extinction spectrum measured on a liquid dispersion of MoS2 nanosheets. The concentration measurement is based on the size-independence of the low-wavelength extinction coefcient, while the size and thickness measurements rely on the effect of edges and quantum connement on the optical spectra. The resultant controllability of concentration, size and thickness facilitates the preparation of dispersions with pre-determined properties such as high monolayer-content, leading to rst measurement of A-exciton MoS2 luminescence in liquid suspensions. These techniques are general and can be applied to a range of two-dimensional materials including WS2, MoSe2 and WSe2.
1 Centre for Research on Adaptive Nanostructures and Nanodevices (CRANN), Trinity College Dublin, Dublin 2, Ireland. 2 School of Physics, Trinity College Dublin, Dublin 2, Ireland. 3 School of Chemistry, Trinity College Dublin, Dublin 2, Ireland. 4 Institut fr Festkrperphysik, Technische Universitat Berlin, Hardenbergstra 36, 10623 Berlin, Germany. 5 Ernst Ruska Center for Microscopy and Spectroscopy with Electrons, Research Center Jlich, 52425 Jlich,
Germany. Correspondence and requests for materials should be addressed to J.N.C. (email: mailto:[email protected]
Web End [email protected] ).
NATURE COMMUNICATIONS | 5:4576 | DOI: 10.1038/ncomms5576 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications 1
& 2014 Macmillan Publishers Limited. All rights reserved.
DOI: 10.1038/ncomms5576
Edge and connement effects allow in situ measurement of size and thicknessof liquid-exfoliated nanosheets
ARTICLE NATURE COMMUNICATIONS | DOI: 10.1038/ncomms5576
Over the last few years the study of two-dimensional (2D) nanomaterials has become an important area of nanoscience14. The palette of 2D materials currently
under study has expanded from graphene3,5, to include transition metal dichalcogenides (TMDs) such as MoS2 and WSe2, layered transition metal oxides such as MnO2 and TiTaO5 and a host of other interesting structures such as GaS, germanane and Bi2Te3 (refs 1,2,4,6) These materials are diverse, including metals, semiconductors, insulators or superconductors1,4,7, and display a range of interesting properties from thickness-dependent bandgaps4 to catalytic activity1. These properties make them useful for both fundamental studies and applications in areas as diverse as optoelectronics, electrochemistry and medicine.
While 2D materials can be grown directly8, they are generally obtained by exfoliation of layered crystals. This has long been possible by mechanical exfoliation, leading to samples of very high quality, but at very low throughput911. When larger production rates are required, chemical methods1215, often based on ion intercalation, have been used to exfoliate layered crystals in liquids2. However, even though these methods result in large quantities of monolayers, they are time consuming, involving harsh chemical treatments, which must be carried out in an inert atmosphere.
More recently, a much simpler method, liquid phase exfoliation (LPE), has been reported1627. This method involves the sonication18 or shearing27 of layered crystals in certain solvents or solutions of surfactants or polymers. It results in the exfoliation of the layered crystal to give large numbers of 2D nanosheets, which are stabilized by interaction with the liquid. The resultant dispersions can be easily processed into lms, coatings or composites: systems which are ideal for applications in a range of areas from batteries28,29 to photodetectors30 to reinforced materials.21,25,31 This method is general and has been used to give exfoliated dispersions of graphene16,17,20, BN,18,23,25 TMDs such as MoS2 and WS218,19,24,26,29,32, transition metal oxides such as
MnO2 (ref. 29) and MoO3 (ref. 33), as well as more exotic structures such as Ti3C2F2 nanosheets34 or functionalized-layered double hydroxides35. In fact, we expect this method to be applicable to any layered compound, where the layers are bound predominately by van der Waals interactions.
While LPE is a versatile and useful technique, it has some notable disadvantages. First, optical characterization of nanosheet dispersions is hampered by the presence of a scattering background, which depends sensitively on the size of the dispersed nanosheets18,24. As such, it is not clear how to dene an intrinsic extinction coefcient, making even concentration measurements challenging.
Moreover, LPE gives nanosheets, which are polydisperse both in thickness and lateral size. While lateral size separation is possible24,36, separation by thickness is more challenging. In addition, measurement of nanosheet size is tedious, requiring time-consuming statistical microscopic analysis. While approximate in situ measurements of lateral size can be made optically37, no in situ method for nanosheet thickness measurement exists. To measure thickness, it is necessary to deposit nanosheets on surfaces, avoiding aggregation and use statistical Raman or atomic force microscopy (AFM)38. This can be very time consuming if a mean over many nanosheets is required. Ultimately, a simple method to separate nanosheets by size and thickness would be very useful. More importantly, a fast in situ method to measure both lateral size and thickness of nanosheets is urgently required.
Here we address these points. We demonstrate size-selection techniques which give fractions with optical extinction spectra which vary systematically with both nanosheet size and thickness. By combining the spectroscopic analysis with statistical
microscopic analysis, we generate quantitative relationships between spectral properties and nanosheet dimensions. Quantifying these effects allows an extinction spectrum to be used to obtain not only the nanosheet concentration but also the nanosheet length and thickness. The ability to control size and thickness is very useful, facilitating for example the preparation of monolayer-rich dispersions. Critically, we nd this methodology to be general to a range of 2D materials.
Results
Size selection of MoS2 nanosheets. To produce dispersions of
MoS2 nanosheets with varying thickness and lateral size distributions from the same stock sample, we used a simple centrifugation technique based on band sedimentation (BS, Fig. 1a). A stock dispersion of the surfactant-exfoliated29 nanomaterial was layered on top of a race layer of higher density and subjected to a short (typically 1040 min) centrifugation using a normal benchtop centrifuge. The centrifugation leads to the spreading of the material through the vial such that nanosheet mass increases going from top to bottom39. Fractionation then allows the collection of size-selected samples. Similar techniques have previously been described in literature to sort carbon nanotubes40,41, graphene oxide nanosheets42 and nano-particles43 by their lateral dimensions. While the higher density of the race layer is normally achieved using a density gradient medium, we use a combination of water and deuterated water to minimize the additive content and avoid potential interactions between gradient medium and MoS2.
After the BS centrifugation, B6 mm deep fractions were collected from the vial, where the smallest, slowest sedimenting species are found in the top fraction (F1). We measured extinction spectra for each fraction. To distinguish it from the true absorbance, Abs, we will refer to the extinction as Ext, where T 10 Ext (T is the optical transmittance). The normalized
extinction spectra of a typical set of fractions (Fig. 1b) display the excitonic transitions typical of MoS2 (ref. 7). However, we nd that they show very distinct and clear changes that obviously reect the different size distributions of the MoS2 nanosheets in the dispersion (Supplementary Fig. 1). The extinction-weighted sum of the individual extinction spectra of the fractions matched well to the stock dispersion (Supplementary Fig. 2) conrming that the changes in the extinction spectra indeed reect the separation process.
In Figure 1b, we see very pronounced spectral changes from fraction to fraction. These changes were quantied by plotting the ratio of extinction at the B-exciton peak (605 nm) to that at the local minimum at 345 nm, ExtB/Ext345 (Fig. 1c). We observe a considerable change with a fourfold increase in this ratio occurring from F1 to F7. Since no such observation has been made when exploring the extinction spectra of lms of restacked chemically exfoliated MoS2 of different nanosheet thicknesses14, this strongly suggests that the spectral changes shown in Fig. 1b,c are related to changes in nanosheet lateral size. This implies that the extinction spectra contain quantitative information on the lateral dimensions of the nanosheets.
In addition to the obvious spectral changes, it is clear that the position of the A-exciton, lA, varied from fraction to fraction.
Because the extinction spectra for MoS2 dispersions include a contribution from a size-dependent scattering background18, we found lA using the second derivative of the extinction spectra (Supplementary Fig. 3). The resultant peak position is plotted in Fig. 1d, showing a clear trend versus fraction number (Fig. 1d). This is consistent with red-shifting of the peak for thicker nanosheets (that is, in higher fractions) such that lA increases as the number of layers per nanosheet, N, increases. Such behaviour
2 NATURE COMMUNICATIONS | 5:4576 | DOI: 10.1038/ncomms5576 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications
& 2014 Macmillan Publishers Limited. All rights reserved.
NATURE COMMUNICATIONS | DOI: 10.1038/ncomms5576 ARTICLE
a
b
2
F1
F2 F3
F4
F5
F7
F6
Sedimentation velocity
F1 F2
F3
F4
F5
F7
F6
Ext (a.u.)
Large and thick F1
F2 F3 F4 F5 F6 F7
B
A
1
Small and thin
0
300 450 600 750 900
Wavelength (nm)
c
d
680
1.2
675
Ext B/Ext 345
0.8
A (nm)
670
0.4
665
Nanosheet size
0.0
Nanosheet size
1 2 3 4 5 6 7
660
1 2 3 4 5 6 7
Fraction
Fraction
Figure 1 | MoS2 band sedimentation and size-dependent extinction spectra. (a) Experimental setup for band sedimentation centrifugation involving layering a nanomaterial stock dispersion on top of a race layer. Centrifugation leads to spreading of the material throughout the vial and separation of the nanosheets according to their sedimentation velocities and so their size. Fractions as indicated are withdrawn from top to bottom. (b) Extinction spectra of the fractions normalized to the local minimum at 345 nm. The positions of the A- and B-excitons are marked. (c) Ratio of extinction at B-exciton to that at 345 nm, ExtB/Ext345 plotted versus fraction number. (d) Peak position (wavelength) of the A-exciton, lA, as a function of fraction number. We propose that lA and ExtB/Ext345 can be used as metrics for ake thickness and length, respectively.
has been observed for a number of TMDs and is due to connement effects14,44,45. This implies that, in addition to lateral size information, the extinction spectra contain quantitative information on the thickness of the nanosheets.
Differentiating absorbance from scattering. However, before any quantitative information can be extracted from the extinction spectra, it is important to realize that such spectra include contributions from both absorbance and scattering. In fact, scattering is known to be signicant for dispersions of nanosheets18, especially those with large lateral size24. To assess the effects of scattering, we prepared a set of MoS2 dispersions with a range of ake sizes. The concentration was measured by ltration and weighing to allow the calculation of extinction (as well as absorption and scattering) coefcients (Supplementary Fig. 4). Extinction spectra were measured and converted to extinction coefcient (e) spectra as shown in Fig. 2a (N.B. Ext eCl, where C
is the concentration and l is the cell length). We used an integrating sphere to differentiate the contributions of absorbance and scattering, leading to the absorption (a) and scattering (s)
coefcient spectra shown in Fig. 2b,c (N.B. e(l) a(l) s(l)). It
is clear from these spectra that scattering makes a signicant contribution to the extinction spectra. For l4700 nm, spl n, with n roughly in the range 14 as suggested previously18,24,46.
However, for lo700 nm, s(l) is broadly similar in shape to a(l). This is important because, as a result, a(l) and e(l) are also similar in shape. This means that any metrics extracted from an extinction spectrum will reect the information contained in the absorption spectrum. To test this, we extracted lA from both extinction and absorbance spectra, plotting one versus another for a range of fractions as shown in Fig. 2d. We also plotted ExtB/
Ext345 versus AbsB/Abs345 in Fig. 2e. For all but the largest fractions (that is, F6 and F7), we nd good scaling between the values extracted from extinction and absorption spectra. This
indicates that, even though scattering is always present, information encoded in an absorption spectrum can be effectively extracted from the extinction spectrum.
The effect of nanosheet length on optical spectra. To test whether the extinction spectrum contains useful information about nanosheet length, we characterized a number of fractions using transmission electron microscopy (TEM). Representative TEM images of dispersions which are expected to contain large and small nanosheets are depicted in Fig. 3ad. These images clearly show the expected size differences. To quantify these effects, we performed statistical analysis of nanosheet lengths for both band-sedimented dispersions and dispersions prepared by conventional centrifugation at different rates (Supplementary Figs 57). We note that BS has the clear advantage of producing much narrower distributions (Supplementary Fig. 7). However, homogenous centrifugation results in larger volumes and so larger quantities of separated materials. We found that the fractions described above contained nanosheets with mean lengths which varied from B60 (F1) to 360 nm (F6), although considerably larger akes (mean length up to 600 nm) can be made by adjusting BS conditions (that is, centrifuging at 2k r.p.m., 10 min).
Before discussing the possibility of developing a length metric, it is worth investigating how the extinction, absorbance and scattering coefcients depend on nanosheet length. Interestingly, the data in Fig. 2a suggests that when l 345 nm, e is relatively
invariant with fraction number and so with L. In Fig. 3e, we plot e, a and s (all at l 345 nm) versus L. We nd e at l 345 nm to
be dominated by absorption and to be invariant with length with a mean of /eSE69 ml mg 1 cm 1 (Supplementary Fig. 8). This allows extinction spectra to be used to estimate the nanosheet concentration for dispersions of any ake length (for Lo300 nm at least). Previously, this was not possible because the inuence of the size-dependent scattering background was unknown18,24.
NATURE COMMUNICATIONS | 5:4576 | DOI: 10.1038/ncomms5576 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications 3
& 2014 Macmillan Publishers Limited. All rights reserved.
ARTICLE NATURE COMMUNICATIONS | DOI: 10.1038/ncomms5576
To assess the possibility of using ExtB/Ext345 as a metric for length, we plot this parameter versus mean nanosheet length, L, for a range of size-selected dispersions in Fig. 3f. We see a clear
increase in ExtB/Ext345 with increasing L, indicating that this ratio can be used as a metric for L. The ratio AbsB/Abs345, calculated from the true absorbance spectra follows the same trend in line with the data in Fig. 2e.
We propose that these size-dependent spectral changes reect the effect of ake edges on the local electronic structure, density of states and hence local optical absorption coefcient of the nanosheets47. This effect may be due to structural relaxations or the misalignment of stacked monolayer edges. In any case, the observed absorption spectrum will be the sum of edge and centre contributions. Because the population ratio of edge to centre atoms increases with decreasing nanosheet size, we expect the spectral shape to be size dependent. We can model this behaviour by treating the akes as consisting of edge (E) and centre (C) regions (Fig. 3f inset), each of which has a well-dened absorption coefcient (that is, aE and aC). Modelling the nanosheets as arbitrary 2D shapes with long dimension, L, and aspect ratio, k (k length/width, Supplementary Note 1), we can
take the area-weighted sum of centre and edge absorption coefcients to derive an expression for the average effective nanosheet extinction coefcient:
a aC 1
2x
L k 1
100
80
F1 F3 F4 F6
(ml mg1 cm1 )
60
40
20
Extinction
0
100
80
F1 F3 F4 F6
(ml mg1 cm1 )
1
where Da aE aC and x is the width of the edge region.
To test this, we plot the absorbance coefcient at both the A- and B-exciton versus the inverse nanosheet length in Fig. 3g. We observed good linearity as predicted by equation (1) so long as L460 nm, below which saturation occurs, consistent with small-ake absorbance being dominated by edges. The t implies values of aC of 311 and 382 ml mg 1 cm 1 for the A-and B-excitons, respectively, while saturation implies equivalent values for aE of 111 and 171 ml mg 1 cm 1. Because TEM analysis shows kE2 for all nanosheet lengths (Supplementary Fig. 5), we can use the ts, coupled with equation (1), to estimate x 127 nm. This value is larger than would be expected for
effects solely due to electronic edge states, suggesting more complex phenomena to be at work. However, it is worth noting that scanning tunnelling microscopy measurements on MoS2 on
graphite have shown a distinct edge region at least 5 nm thick48. Nevertheless, the effects described here may not be universal but perhaps specic to nanosheets surrounded by a weakly interacting environment (for example, surfactant micelle or solvent solvation shell).
To conrm the presence of a distinct edge region, X-ray photoelectron spectroscopy (XPS) was performed on a range of lms prepared from nanosheets of different sizes. No systematic changes in the Mo core-level spectra (Supplementary Fig. 9) were detected. However, in addition to the expected 2H component of the S2p core-level spectra, as long as we investigate freshly prepared samples, we observe an extra component that cannot be identied with known morphologies, for example 1 T MoS2 (Fig. 3h) (also Supplementary Fig. 10). Critically, the intensity of this additional component increases with decreasing ake length allowing us to associate it with the edge region. Then, the fraction of the S2p signal associated with this component will equal the fraction of S atoms associated with the edge region; NS,E/NS,T.
This ratio is plotted as a function of ake length in Fig. 3i. The fraction of S atoms within a distance x from the edge is given by
NS;E
NS;T
2x
L 1 k 1
Da aC
60
40
20
Absorbance
Scattering
0
50
40
F1 F3 F4 F6
(ml mg1 cm1 )
30
20
10
0
300 400 500 600 700 800
Wavelength (nm)
0.0 0.4 AbsB/Abs345
0.8 1.2
678
F6
1.2
F6
Extinction A(nm)
670
Ext B/Ext 345
0.8
0.4
662
F1
F1
0.0
660 668 676
Abs A (nm)
Figure 2 | Extinction, absorbance and scattering spectra. (a) Wavelength dependence of optical extinction coefcient, e, for fractions F1, F3, F4 and
F6. NB e is dened by T 10 eCl where T is the transmittance, C is the
MoS2 concentration and l the cell length. e can be split into contributions from absorption, a, and scattering, s, such that e a s. (b,c) Wavelength
dependence of (b) optical absorption coefcient, a, and (c) optical scattering coefcient, s. (d) A-exciton position measured from the extinction spectra (Fig. 2a) plotted versus that measured from the absorption spectra (Fig. 2b) for fractions F1F6. (e) ExtB/Ext345 (measured from the extinction spectra, Fig. 2a) plotted versus AbsB/Abs345 (measured from the absorption spectra, Fig. 2b) for fractions F1F6.
2
This expression describes the data in Fig. 3i rather well, giving a value of x 2.70.5 nm. We note that this value for x is lower
than the one quoted above, suggesting that XPS probes edge
2x L
4 NATURE COMMUNICATIONS | 5:4576 | DOI: 10.1038/ncomms5576 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications
& 2014 Macmillan Publishers Limited. All rights reserved.
NATURE COMMUNICATIONS | DOI: 10.1038/ncomms5576 ARTICLE
properties which are distinct to those seen by absorbance measurements.
To further illustrate differences in electronic structure between edge and centre of MoS2 nanosheets, we have performed scanning
TEM (STEM) imaging (Fig. 3jk) and low-loss STEM electron energy-loss spectroscopy (EELS, Supplementary Figs 11 and 12). Moving inward from the nanosheet edge (Fig. 3k), the EEL spectra (Fig. 3l) exhibited gradual changes in the energy-loss regions between 2 and 10 eV. These changes reect differences in electronic structure near the ake edge compared with the centre. We examined these changes via the ratio of EELS intensities at two energies, for example, 2.8 and 6.4 eV, I2.8eV/I6.4eV. These
specic positions were chosen, as they show the largest changes in
the spectra with distance from the edge. We have calculated this
ratio for a number of spectra, measured at a range of positions on three different nanosheets, as a function of distance from nanosheet edge as shown in Fig. 3m. We took care to choose regions of uniform thickness to exclude effects from thickness variations in the EELS. This data clearly shows I2.8eV/I6.4eV to fall
off with increasing distance from the edge before saturating for spectra collected at a distance of 48 nm from the ake edge. This suggests the presence of a distinct edge region with thickness of xB8 nm in good agreement with the optical measurements (taking into account limitations to the spatial resolution). However, this result has to be interpreted with caution, since in this region of the low-loss spectra the exact origin of the peaks remains uncertain.
The strong effect of nanosheet edges on electronic properties is also consistent with recent reports, which show MoS2 in the vicinity of edges48,49 or grain boundaries50 to have electronic properties distinct from the central regions. Incidentally, this suggests that this approach could be used to measure grain size in chemical vapour deposition-grown MoS2.
Length metric based on nanosheet edge effects. We can use our model to understand the size-dependent changes to the shape of absorption spectra. We represent the spectral shape by the ratio of absorbance intensities at two distinct wavelengths, l1 and l2.
Using equation (1), we can express this as
Absl1 Absl2
aC
a
F1 b d
F1 F6
170 nm
207 nm
c F6
100
345 nm
2H MoSEdge S S 2p
20 nm
, ,
(ml mg1cm1)
l1L 2xk 1Dal1
aC
l2L 2xk 1Dal2
3
Because of the linear relationship between ExtB/Ext345 and AbsB/ Abs345 (Fig. 2e), we can re-write this as
ExtB Ext345
aC
10
55 nm
0 100 200 300 400
Length, L (nm)
Intensity
114 nm
345 nmL 2xk 1Da345 nm
4
Equation (4) can be used to t the data in Fig. 3f, showing very
lBL 2xk 1DalB
aC
1.6
1.2
x
0.8
Ratio
0.4
Figure 3 | Length metric and edge effects. (a,b) Representative TEM images of slowly sedimenting MoS2 nanosheets (small akes, F1, (a) scale bar, 100 nm, (b) scale bar, 10 nm). (c,d) Representative TEM images of faster sedimenting MoS2 nanosheets (large akes, F6, (c) scale bar, 1 mm, (d) scale bar, 100 nm). (e) Extinction (e), absorption (a) and scattering (s)
coefcients at 345 nm plotted versus nanosheet length. The line represents /eS 69 ml mg 1 cm 1. (f) Ratio of extinction at B-exciton to that at
345 nm, ExtB/Ext345, plotted versus the lateral dimensions of the ake (expressed as mean length, L, obtained by statistical TEM analysis). The line is a t to equation (4). Also shown is the equivalent data taken from the absorbance spectra (AbsB/Abs345). The inset schematically shows the division of a nanosheet into edge and central regions. (g) Absorption coefcient, a, at both A- and B-excitons plotted versus inverse nanosheet length. The dashed lines are ts to equation (1). (h) Fitted XPS S2p core-level spectra of ltered MoS2 dispersions with different mean ake lengths.
The additional component at higher binding energies is attributed to edge S. (i) Fraction of S2p signal associated with edge S as a function of ake length. This fraction is equal to the ratio of edge S to total S atoms. The line represents a t to equation (2) and yields the width of the edge region to be x 2.70.5 nm. (j) Scanning transmission electron microscopy (STEM)
image of MoS2 nanosheets (scale bar, 20 nm). (k) STEM image of the region marked by the box in j showing the edge region of a typical MoS2 nanosheet (scale bar, 5 nm). The boxes indicate the regions over which EEL spectra were acquired and analyzed. (l) Summed EEL spectra, normalized to the zero-loss peak, of the regions marked by the boxes in k (same data set as Supplementary Fig. S12c). The EEL spectra exhibited gradual changes when moving from the edge to the centre. (m) Plot of EELS intensity ratio at2.8 eV to that at 6.4 eV (as indicated in l) as a function of distance from the edge. Data from three different regions are shown. The intensity ratio saturates at B8 nm from the edge.
Ext /Ext Abs /Abs
0.2 20 100 800
166 164 162 160 158
1 10 100 400
Length, L (nm)
Binding energy (eV)
40
(ml mg1cm1)
100
30
20
Ratio, N S,E/N S,T(%)
B-exciton
10
10
A-exciton
x=2.7 nm
0 0.00 0.01 0.02 0.03 0.04
Inverse length, 1/L (nm1)
Length, L (nm)
Edge 2 nm 4 nm
9 nm
6.4
2.8 Centre
2.5
2.0
x~8 nm
Intensity (a.u.)
9 nm
Ratio I 2.8 eV/I 6.4 ev
4 nm
1.5
2 nm
Edge
Edge
1.0
2 4 6 8 10
0 4 8 12 16
Energy loss (eV)
Distance from edge (nm)
NATURE COMMUNICATIONS | 5:4576 | DOI: 10.1038/ncomms5576 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications 5
& 2014 Macmillan Publishers Limited. All rights reserved.
ARTICLE NATURE COMMUNICATIONS | DOI: 10.1038/ncomms5576
both surfactant-tip and surface-tip interactions contribute to the apparent height of the nanosheets, making N assessment difcult. To resolve this, we utilized the fact that incompletely exfoliated nanosheets often display terraces separated by steps associated with ake edges (Fig. 4d inset). By analyzing the apparent AFM height on a large number of steps over many akes27 and plotting the step height in ascending order (Fig. 4d), it is clear that the step height is always a multiple of 1.9 nm. Even though this is larger than expected for monolayer MoS2, the absence of smaller step heights implies surfactant-exfoliated MoS2 to display apparent monolayer heights of 1.9 nm (cf 1.1 nm for chemically exfoliated MoS2)14. Furthermore, the thinnest akes we have observed have an apparent height of 3 nm, consistent with a monolayer height of1.9 nm plus B1 nm surfactant under the akesUnequivocal evidence that the nanosheets with an apparent
height of 3 nm are monolayered MoS2 can be obtained using photoluminescence (PL) and Raman spectroscopy, which allows identication of mono-, bi- and tri-layer MoS2 (refs 38,44). For this, we relocated the sample area characterized by AFM (Fig. 4a,b) to a Raman microscope to optically characterize those akes with known AFM thickness. Raman mapping, plotted as intensity of the A1g mode in Fig. 4e, shows the presence of many
MoS2 akes on the substrate in these regions. Critically, some of these akes also display PL (Fig. 4f). The observed PL (and Raman spectra) from akes with a height of B3 nm was always consistent with monolayered MoS2 (Fig. 4c,g and Supplementary Figs 2022). In contrast, slightly thicker akes (for example, 57 nm in height), showed weaker PL with a clear shoulder at 620 nm, consistent with bi- and few-layered species38,5153.
This combination of AFM, Raman and PL spectroscopy clearly shows that surfactant-exfoliated monolayers display an apparent height of 3 nm with every additional monolayer contributing an extra 1.9 nm. This in turn allows the conversion of the mean AFM
PL
good agreement, at least in the size range of 70350 nm. Once the t parameters are known, equation (4) can be rearranged to give a quantitative relationship between L and ExtB/Ext345:
Lmm
3:5ExtB=Ext345 0:14
11:5 ExtB=Ext345
5
By assessing the root-mean-square relative difference between data and t we estimate the error in L to be o10%. This is important and it allows ExtB/Ext345 to be used to assess ake length for MoS2 suspended in liquids simply by measuring the extinction spectrum. It works effectively for nanosheets in the size range 70oLo350 nm, which is almost exactly the range of nanosheets typically produced by LPE. For larger nanosheets, a different metric, based on the scattering exponent n can be used (Supplementary Figs 1316 and Supplementary Note 2).
Nanosheet thickness metric based on connement effects. While a spectroscopic method to determine nanosheet length is undoubtedly important, even more useful would be an in situ method to assess thickness. As discussed above, it is clear that the position of the A-exciton peak in the absorbance spectrum has the potential to provide such a metric14,44. However, the number of layers per ake, N, must be measured before the relationship between peak position and N can be quantied.
To do this, we deposited nanosheets from a number of fractions onto Si/SiO2 wafers for characterization by AFM (Fig. 4a,b). In this way, we measured mean thicknesses for a large number of nanosheets across a number of fractions (Fig. 4c and Supplementary Figs 1719).
However, conversion of the measured height into the actual number of monolayers per ake, N, is challenging due to adsorbed surfactant on both akes and substrate. This means
1.2
Intensity (a.u.)
0.8
0.4
Raman
0.0 0 15 30 45 60
Wavelength (nm)
30
10 Ext metric
Ext/AFM Abs/AFM Mak et al.51 PL
10
Height (nm)
13.3
Step height (nm)
11.4
Abundance (%)
Number of layers,
8
9.5
20
6
7.6
4
5.7
10
3.8
2
1.9 nm
1.9
1
0 1 2 3 4 5 6 7 8 9
0 0.0 0.1 0.2 Position (m)
0.3 0.4
650 660
A (nm)
670 680
Sample number
Layer number, N
0.0 600 650 700
Figure 4 | Thickness metric. (a) Representative overview AFM images of a surfactant-exfoliated MoS2 dispersion deposited on Si/SiO2 wafers (scale bar, 1 mm). (b) Zoomed-in AFM images of the regions indicated in a. (c) Height proles of the nanosheets in (b). (d) Heights of steps observed on deposited
MoS2 nanosheets such as that displayed in the inset (scale bar, 250 nm). The step height is found to be a multiple of 1.9 nm. (e) Raman (integrated A1g phonon area, scale bar, 1 mm) and (f) PL maps (excitation 532 nm, integrated area from 640700 nm, scale bar 1 mm) of the region shown in a.
(g) Photoluminescence spectra of the areas marked by circles (colour coded). The blue circle and spectrum, respectively, is associated with a ake of apparent height 3 nm (Fig. 4c). Inset: zoom-in of PL from multi-layered akes marked by red and green circles associated with akes of apparent thickness 57 nm (Fig. 4c). (h) Example (fraction F2) of a layer number histogram after conversion of AFM height to number of layers. (i) Plot of the mean number of layers as obtained from AFM thickness analysis versus the wavelength associated with the A-exciton measured from both extinction and absorbance spectra. The vertical error bars represent the standard error of the AFM height distribution. The red lled diamond represents free-standing micromechanically cleaved MoS2 monolayer, where lA was obtained from the PL peak position. The experimental ndings are consistent with literature data on the photoluminescence of free-standing MoS2 extracted from Mak et al.51 NB proles in c are colour coded with the lines in b.
6 NATURE COMMUNICATIONS | 5:4576 | DOI: 10.1038/ncomms5576 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications
& 2014 Macmillan Publishers Limited. All rights reserved.
NATURE COMMUNICATIONS | DOI: 10.1038/ncomms5576 ARTICLE
height obtained by statistical analysis of a given dispersion drop-cast on Si/SiO2 wafers to the actual number of layers. This is depicted in Fig. 4h for a BS fraction, which optical measurement showed to have a low mean nanosheet thickness (that is, F2 with A-exciton position 666 nm 1.86 eV).
These results allow us to use AFM to measure the mean value of N in different fractions and so quantify the relationship between the mean number of monolayers per nanosheet, N, and the measured A-exciton position, lA. We plot this data in Fig 4i for lA taken both from extinction and absorption spectra. In both cases, the data are very similar, showing a well-dened relationship between N and lA. The data point for the monolayer was obtained from determining the A-exciton energy from the PL of free-standing micromechanically cleaved MoS2 (Supplementary
Fig. 23, in absence of surfactant). We can test these results by comparing them to literature data51 for A-exciton position for mono-, bi- and tri-layer mechanically exfoliated MoS2, nding very close agreement. This suggests any solvatochromic effect54 associated with the presence of adsorbed sodium cholate to be small as conrmed by additional experiments (Supplementary Fig. 24).
The data in Fig. 4i clearly show an exponential relationship between N and lA. Fitting the data where lA is taken from the extinction spectrum gives
N2:3 1036e 54;888=lA 6
with lA in nanometre. This expression can be used to nd the mean number of monolayers per nanosheet directly from the extinction spectrum of a MoS2 dispersion. However, we note that for NB10, the extinction and absorbance data begin to diverge, as scattering becomes more important. Thus, while equation (5) is only accurate for No10, this is not a serious limitation as LPE typically gives dispersions with No10. In addition, because the properties of MoS2 become bulk like as N approaches 10 (refs 38), knowledge of the exact thickness in this regime is unnecessary.
It is important to demonstrate that these metrics are indeed independent of each other. We do this by analyzing dispersions prepared in a way which allows thickness and length to be varied independently. Such analysis (Supplementary Note 3; Supplementary Figs 25 and 26) shows that ExtB/Ext345 and lA are not intrinsically linked (although there may be a relationship between mean nanosheet thickness and length, which is due to the exfoliation mechanism, see below). In addition, we have shown (Supplementary Fig. 27) that the metrics work well even at the highest dispersion concentrations. This is an important result, which makes it possible to determine both mean length and number of layers for solution-processed MoS2 nanosheets using two metrics extracted from a simple extinction spectrum, which is measureable in any laboratory.
Applying length and thickness metrics. We can use these metrics to assess the dimensions of akes in a wide range of dispersions produced under a range of conditions including simple homogenous centrifugation at different rates as well as samples that were fractionated by BS. Shown in Fig. 5a, is a graph of extinction ratio ExtB/Ext345 plotted versus lA for 450 dispersions. It is clear that these data all fall on the same master curve. We can use equations (5 and 6) to transform Fig. 5a into a graph of L versus N (Fig. 5b). This curve is interesting, showing a clear correlation between lateral size and thickness. This is not because the metrics are correlated. Rather, it is due to the greater interlayer binding energy associated with larger akes: they are harder to exfoliate and so are thicker on average. Such a correlation has previously been observed for liquid-exfoliated MoO3 nanosheets33 and conrmed in this work on ake by ake
measurements of MoS2-sodium cholate (SC) (Supplementary Fig. 28). Importantly, Fig. 5b shows that dispersions can be produced with mean values of N close to 1.
The ability to both control and easily measure nanosheet size and thickness will be extremely useful, facilitating the processing of materials for both applications and basic research. We demonstrate the application of these techniques in both of these areas. First, we demonstrate the utility of accurate size control and measurement by preparing hydrogen-evolution catalysts from solution-exfoliated MoS2. The sites responsible for the catalysis of hydrogen evolution by MoS2 are known to reside on the ake edges55, making small akes desirable and illustrating the need for size control. We prepared two dispersions using distinct centrifugation protocols. The measured extinction spectra were used to determine the mean lateral size of nanosheets (190 and
1.5
Ext B / Ext 345 nm
0.3
Length, (mm)
0.2
1.0
0.5
0.1
0.0 660 670 680
0.05 1 2 4 6 8 10
A (nm)
Thickness, N
0
0.5
120 mV per dec
J (mA cm2 )
Overpotential (V)
1
0.4
L=190 nm
L=60 nm
0.3
2
75 mV per dec
0.2
L=190 nm
L=60 nm
3 0.5 0.3 0.1
0.2 1 J (mA cm2)
2
V v RHE (V)
600
7
Excitation em=650 nm
6
Emission ex=435 nm
550 Raman - OH
5
ex (nm)
Intensity (a.u.)
C
A
500
4
3
B
450
2
400
1
620 640
em (nm)
660 680
0 400 500 600 700
(nm)
Figure 5 | Use of the metric for applications and fundamental studies. (a,b) Map of extinction metrics for length and thickness for a number of fractions obtained by band sedimentation under varying centrifugation conditions from various stock dispersions. (a) Raw data from extinction spectroscopy and (b) converted to actual mean length and thicknessby using the calibration equations obtained from spectroscopy and microscopy. (c) Linear sweep voltammograms (5 mVs 1) for lms of length-selected MoS2 on indium tin oxide (ITO) substrates, comparing the electrocatalytic response towards hydrogen-evolution reaction.
Measured potentials were subjected to iR correction (see Supplementary Information). Supporting electrolyte was 0.5 M H2SO4. (d) Overpotential versus current density plots showing Tafel slopes expressed as mV per decade (mV per dec). (e) Photoluminescence excitation contour plot ofa monolayer-rich MoS2-SC dispersion showing the expected A-exciton uorescence at 651 nm. (f) Excitation spectrum of the emission signal collected at 650 nm and emission spectrum excited at 435 nm. A, B and C-excitonic features are clearly identied. The Raman signal of OH was subtracted from the excitation spectrum.
NATURE COMMUNICATIONS | 5:4576 | DOI: 10.1038/ncomms5576 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications 7
& 2014 Macmillan Publishers Limited. All rights reserved.
ARTICLE NATURE COMMUNICATIONS | DOI: 10.1038/ncomms5576
60 nm) as well as the concentration of dispersed material. Vacuum ltration was used to produce thin lms (30 mg cm 2), which were transferred onto indium tin oxide-coated glass substrates and characterized for hydrogen-evolution catalysis (see methods and Supplementary Note 1). A clear size effect is seen (Fig. 5c,d), with considerably lower onset potential and Tafel slope55 observed for the smaller akes compared with larger ones. This demonstrates the potential of our method to facilitate optimized sample preparation for applications of nanosheets.
Furthermore, the ability to produce dispersions with controlled nanosheet dimensions allows the preparation of samples for more fundamental studies. To demonstrate this, we used size selection coupled with analysis via the thickness metric to produce monolayer-rich (that is, with low average N) MoS2 dispersions, which allow the study of solution-phase PL. Shown in Fig. 5e is a PL-excitation contour plot for such a dispersion, which shows the direct band gap luminescence associated with monolayer MoS2 (lem 651 nm). The emission spectrum (lex 435 nm) shows a
narrow peak (full-width half-maximum 23 nm) that can be
tted to a single Lorentzian, consistent with PL from mono-layered MoS2. The PL spectrum is size independent with no apparent edge effect other than reduction of PL intensity for very small nanosheets (Supplementary Note 4 and Supplementary Figs 29 and 30). Fluorescence from few and multi-layered species in the dispersion (with a mean thickness of two layers) cannot be resolved due to the signicantly lower quantum efciency51. The excitation spectrum (after subtraction of Raman mode of water,
lex
Ext (a.u.)
1.5 F1 F2 F3 F4 F5 F6 F7
1.0
651 nm) is depicted in Fig. 5f, clearly revealing signatures of the B and C-excitonic transitions. We note that while the measurement of contour maps and excitation spectra is virtually impossible using micromechanically cleaved MoS2, it is
straightforward in liquid once size selection and measurement
techniques are known.
Extension of metrics to other nanosheet types. The nanosheet extinction metrics described in this paper rely on fundamental principles that both ake edge and degree of exfoliation inuence the electronic structure. This implies that this is a general method that can be used for a wide range of liquid-exfoliated nanosheets. To demonstrate this, we show the same changes to extinction spectra for band-sedimented, surfactant-exfoliated dispersions of WS2 (Fig. 6), MoSe2 and WSe2 (Supplementary Figs 3233).
Almost identical behaviour is observed in all materials although the extinction ratio must be calculated using appropriate wavelengths: for WS2, we use ExtA/Ext295, where A represents the
A-exciton position (for example, Fig. 6ac). The ability to identify well-exfoliated WS2 allowed us to prepare dispersions containing very thin nanosheets (that is, with low lA). A combination of Raman and PL spectroscopy, coupled with AFM (Fig. 6dg) conrmed such dispersions to be rich in monolayers. Compared with MoS2, the WS2 PL (normalized to the Raman 2LA and nearby modes in Fig. 6h) appears signicantly enhanced. In addition, unlike MoS2, the PL associated with WS2 edges was red shifted and more intense than that from the nanosheet centre (Fig. 6h). This suggests that the band gap of the edge region in liquid-exfoliated WS2 is smaller than that of the centre, in agreement with previous results56. Most importantly, neither very small (B50 nm), nor reasonably sized (B300 nm) few-layer species show a notable PL signal further supporting that the nanosheets with a nominal AFM height of 3 nm are monolayered nanosheets.
DiscussionIn conclusion, we have introduced a simple and versatile centrifugation technique based on BS to rapidly sort liquid-suspended TMDs according to their mass using a normal benchtop centrifuge. This process gave a range of fractions, which had signicantly different extinction spectra. Specically, both the energy of the A-exciton and the relative intensity of the B-excitonic transition varied systematically with fraction number (that is, with nanosheet size). These parameters are related to nanosheet thickness and lateral size, respectively. Statistical measurements of nanosheet length and thickness, made using TEM and AFM, allowed us to quantify these relationships. Such quantication gives access to the determination of mean ake length and thickness in one single extinction measurement. In addition, we nd the extinction coefcient at 345 nm to be widely independent of nanosheet thickness and length, allowing the extinction spectrum to be used to measure concentration.
The variations in the MoS2 absorbance and extinction spectra with nanosheet size described above are due to the effects of both connement and nanosheet edges on the electronic structure of the material. Since these phenomena are general to all 2D materials, the extinction metrics described here can be applied to a range of nanosheet types as we demonstrate for WS2, WSe2 and MoSe2.
We believe this to be an important result for a number of reasons. On the one hand, the availability of a simple spectroscopic method to measure both thickness and lateral size will be extremely important and will greatly simplify the basic characterization of dispersions of liquid-exfoliated nanosheets. In addition, these results will facilitate the preparation of liquid-
Height (nm)
A
8
6
0.5
4
2
0.0 300 450 600 750
0 0.2 0.4
0.0Length (m)
Wavelength (nm)
Raman PL
630
A (nm)
626
622
0 1 2 3 4 5 6 7 8
Fraction
1 2 3 4 5 6 7
0.6
5 ML center ML edge
4
Ext A / Ext 295 nm
Norm. intensity
3
0.4
2
0.2
1
0 575 600 625 650
Fraction
Wavelength (nm)
Figure 6 | Metric for WS2. (a) Extinction spectra, normalized to 295 nm, of surfactant exfoliated WS2 fractions after band sedimentation at 2.5k r.p.m.
for 10 min. The A-exciton is labelled. (b) A-exciton wavelength plotted as a function of fraction number. (c) Extinction peak ratio, ExtA/Ext295, plotted versus fraction number. (d) Typical AFM images of deposited WS2 nanosheets (scale bar, 1 mm) and (e) height prole of the nanosheet at the top right (scale bar, 250 nm). (f) Raman and (g) PL intensity map (532 nm excitation) of the same area (scale bar, 1 mm). (h) Representative PL spectra of the nanosheet displayed in e at the centre and in the edge region.
8 NATURE COMMUNICATIONS | 5:4576 | DOI: 10.1038/ncomms5576 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications
& 2014 Macmillan Publishers Limited. All rights reserved.
NATURE COMMUNICATIONS | DOI: 10.1038/ncomms5576 ARTICLE
suspended nanosheets with well-dened length and thickness distributions. This will be extremely important for applications where nanosheet size is crucial, as well as for understanding fundamental physical properties of layered inorganic materials as a function of size (for example, by uorescence spectroscopy in solution). Furthermore, this work highlights the inuence the edge has on the electronic and optical properties of the nanosheet as a whole.
Methods
Sample preparation. Details are presented in the Supplementary Methods. In brief, TMD dispersions (100 ml) were prepared by probe sonicating (Sonics VX-750) the powder (Sigma Aldrich, typical 20 g l 1) in an aqueous SC with the constant weight ratio of SC/TMD 0.3. The resultant raw dispersion was left to
settle overnight and subjected to a pre-centrifugation step (Hettich Mikro 220R centrifuge, xed angle rotor 1016, 750 r.p.m., 60 g) to remove unexfoliated material. Prior to BS, 1 ml of the stock dispersion of the nanomaterial in aqueous SC was layered on top of the race layer containing 5 ml of deuterated water at the bottom and 5 ml of 1:1 mixture of deuterated water and water (equal surfactant concentrations). After centrifugation in a Heraeus Megafuge 16 benchtop centrifuge equipped with a 3,655 swinging bucket rotor, typically (unless otherwise noted) at 5k r.p.m. (4,695 g) for 10 min, the seven fractions were collected from the initial 11 ml liquid from top to bottom to obtain samples with standard size and thickness distributions. To obtain larger akes, conditions were modied: large and thick akes were enriched in a dispersion by rst centrifuging the stock dispersion at 1k r.p.m. (107 g, Hettich Mikro 220R centrifuge, xed angle rotor 1016). The supernatant was then subjected to a second centrifugation at 2k r.p.m. (425 g). The sediment after this centrifugation was collected for BS at 2k r.p.m. for 10 min (1,135 g). To obtain the monolayer-rich dispersion for PLE measurements, the stock dispersion was centrifuged at 5k r.p.m. (2,663 g, 2 h, Hettich Mikro 220R centrifuge, xed angle rotor 1016), the sediment was discarded, the supernatant was again centrifuged at 15k r.p.m. (22,500 g, 2 h, Hettich Mikro 220R centrifuge, xed angle rotor 1195-A). After the second centrifugation step, the sediment was reagitated in 0.1 mg ml 1 SC (reducing the initial volume by 50% to yield a high concentration) and subjected to PL measurements. For XPS and electrochemical measurements, the dispersions were vacuum-ltered using porous cellulose lter membranes. For Raman, PL and AFM, dispersions were drop-casted on Si/SiO2 wafers.
Characterization. Optical extinction was measured on a Varian Cary 5,000 in quartz cuvettes with a pathlength of 0.4 cm. To distinguish between contributions from scattering and absorbance to the extinction spectra, dispersions were measured in an integrating sphere using a home-built sample holder to place the cuvette in the centre of the sphere of a Perkin Elmer Lamda 650 spectrometer (NB cuvettes need to be transparent to all sides). The absorbance spectrum is obtained from the measurement inside the sphere. A second measurement on each dispersion was performed outside the sphere to obtain the extinction spectrum. This allows calculation of the scattering spectrum (extinction-absorbance). Bright eld TEM imaging was performed using a JEOL 2100, operated at 200 kV, while high-resolution TEM was conducted on a FEI Titan TEM (300 kV) on holey carbon grids (400 mesh). Tapping-mode AFM was carried out on a Veeco Nanoscope-IIIa system (Digital Instruments). Raman and PL spectroscopy on substrate was performed using a WITec alpha 300 with 532 nm excitation laser in air under ambient conditions. The PL in solution was acquired on a Fluorolog-3 spectrometer (Horiba Scientic) with a thermoelectrically cooled R928P photomultiplier tube detector. The samples were excited with a 450 W Xe lamp with a double monochromator in excitation (600 grooves per mm, 500 nm blaze grating). XPS was performed under ultra-high vacuum conditions (o5 10 10 mbar), using monochromated Al Ka
X-rays (1,486.6 eV) from an Omicron XM1000 MkII X-ray source and an Omicron EA125 energy analyzer. An Omicron CN10 electron ood gun was used for charge compensation and the binding energy scale was referenced to the adventitious carbon 1s core level at 284.8 eV. Mo 3d and S 2p core-level regions were recorded at an analyzer pass energy of 15 eV and with slit widths of 6 mm (entry) and 3 mm x 10 mm (exit), resulting in an instrumental resolution of 0.48 eV. After subtraction of a Shirley background, the core-level spectra were tted with Gaussian-Lorentzian line shapes and using Marquardts algorithm. STEM imaging and STEM-EELS investigations were carried out using an FEI Titan 60300 Ultimate microscope (PICO) operated at 80 keV, equipped with a high-brightness electron gun, a Cs probe corrector, and a Gatan Quantum postcolumn energy lter system (Ernst Ruska-Centre Juelich). The suspended MoS2 akes were dropped onto lacey carbon-coated copper TEM grids that were then heated up to 120C overnight under vacuum to minimize contamination of the sample. EELS spectra were acquired with a convergence angle of 24 mrad, a collection angle of B28 mrad, a dispersion of 0.01 eV/channel and an energy resolution over vacuum of 0.1 eV. STEM-EELS maps were acquired with 0.01 s acquisition time per spectra per pixel. Subsequently, the spectra were aligned and calibrated using the zero-loss peak. Individual spectra (1,152) were summed to obtain each of the spectra shown in Fig. 3l.
The spectra shown here are representative of a set of 20 STEM-EELS maps that
were acquired over similar regions. For the plot of EELS intensity ratio, I2.8eV/
I6.4eV, in Fig. 3m, spectra in three different regions of interest perpendicular to the ake edge were averaged parallel to the edge. Three sets of EELS maps were analyzed in total: set 1:150 spectra acquired over 4.17 nm 1 nm (direction per
pendicular to the edge of the ake) were summed for each spectrum that was analyzed; set 2:282 spectra acquired over 14.67 nm 0.47 nm (direction perpen
dicular to the edge of the ake) were summed for each spectrum that was analyzed; set 3:66 spectra acquired over 8.34 nm 0.51 nm (direction perpendicular to the
edge of the ake) were summed for each spectrum that was analyzed. The spectra were then normalized to the intensity of the zero-loss peak. Subsequently, the ratio at 2.8 eV in the EELS to that at 6.4 eV as a function of distance from the edge was plotted. Electrochemical characterization consisted of linear sweep voltammetry (2mV s 1) and electrochemical impedance spectroscopy using a three-electrode electrochemical cell and Gamry Reference 3,000 potentiostat. The measurements were performed in 0.5 M H2SO4 solution using a three-electrode electrochemical cell, with a Ag/AgCl (3 M NaCl) reference electrode and graphite rod counter electrode.
References
1. Chhowalla, M. et al. The chemistry of two-dimensional layered transition metal dichalcogenide nanosheets. Nat. Chem. 5, 263275 (2013).
2. Nicolosi, V., Chhowalla, M., Kanatzidis, M. G., Strano, M. S. & Coleman, J. N. Liquid exfoliation of layered materials. Science 340, 6139 (2013).
3. Novoselov, K. S. et al. A roadmap for graphene. Nature 490, 192200 (2012).4. Wang, Q. H., Kalantar-Zadeh, K., Kis, A., Coleman, J. N. & Strano, M. S. Electronics and optoelectronics of two-dimensional transition metal dichalcogenides. Nat. Nanotechnol. 7, 699712 (2012).
5. Geim, A. K. Graphene: status and prospects. Science 324, 15301534 (2009).6. Huang, X., Zeng, Z. Y. & Zhang, H. Metal dichalcogenide nanosheets: preparation, properties and applications. Chem. Soc. Rev. 42, 19341946 (2013).
7. Wilson, J. A. & Yoffe, A. D. Transition metal dichalcogenides discussionand interpretation of observed optical, electrical and structural properties. Adv. Phys. 18, 193335 (1969).
8. Zhan, Y. J., Liu, Z., Najmaei, S., Ajayan, P. M. & Lou, J. Large-area vapor-phase growth and characterization of MoS2 atomic layers on a SiO2 substrate. Small 8, 966971 (2012).
9. Frindt, R. F. single crystals of MoS2 several molecular layers thick. J. Appl. Phys. 37, 19281929 (1966).
10. Novoselov, K. S. et al. Two-dimensional atomic crystals. Proc. Natl. Acad. Sci. USA 102, 1045110453 (2005).
11. Radisavljevic, B., Radenovic, A., Brivio, J., Giacometti, V. & Kis, A. Single-layer MoS2 transistors. Nat. Nanotechnol. 6, 147150 (2011).
12. Murphy, D. W. & Hull, G. W. Monodispersed tantalum disulde and adsorption complexes with cations. J. Chem. Phys. 62, 973978 (1975).
13. Joensen, P., Frindt, R. F. & Morrison, S. R. Single-Layer MoS2. Mater. Res. Bull.
21, 457461 (1986).
14. Eda, G. et al. Photoluminescence from chemically exfoliated MoS2. Nano Lett. 11, 51115116 (2011).
15. Zeng, Z. Y. et al. Single-Layer semiconducting nanosheets: high-yield preparation and device fabrication. Angew. Chem. Int. Ed. 50, 1109311097 (2011).
16. Blake, P. et al. Graphene-based liquid crystal device. Nano Lett. 8, 17041708 (2008).
17. Bourlinos, A. B., Georgakilas, V., Zboril, R., Steriotis, T. A. & Stubos, A. K. Liquid-phase exfoliation of graphite towards solubilized graphenes. Small 5, 18411845 (2009).
18. Coleman, J. N. et al. Two-dimensional nanosheets produced by liquid exfoliation of layered materials. Science 331, 568571 (2011).
19. Cunningham, G. et al. Solvent exfoliation of transition metal dichalcogenides: dispersability of exfoliated nanosheets varies only weakly between compounds. ACS Nano 6, 34683480 (2012).
20. Hernandez, Y. et al. High-yield production of graphene by liquid-phase exfoliation of graphite. Nat. Nanotechnol. 3, 563568 (2008).
21. Khan, U. et al. Polymer reinforcement using liquid-exfoliated boron nitride nanosheets. Nanoscale 5, 581587 (2013).
22. Khan, U., ONeill, A., Lotya, M., De, S. & Coleman, J. N. High-concentration solvent exfoliation of graphene. Small 6, 864871 (2010).
23. Lin, Y., Williams, T. V. & Connell, J. W. Soluble, exfoliated hexagonal boron nitride nanosheets. J. Phys. Chem. Lett. 1, 277283 (2010).
24. ONeill, A., Khan, U. & Coleman, J. N. Preparation of high concentration dispersions of exfoliated MoS2 with increased ake size. Chem. Mater. 24, 24142421 (2012).
25. Zhi, C. Y., Bando, Y., Tang, C. C., Kuwahara, H. & Golberg, D. Large-scale fabrication of boron nitride nanosheets and their utilization in polymeric composites with improved thermal and mechanical properties. Adv. Mater. 21, 28892893 (2009).
26. Zhou, K. G., Mao, N. N., Wang, H. X., Peng, Y. & Zhang, H. L. A mixed-solvent strategy for efcient exfoliation of inorganic graphene analogues. Angew. Chem. Int. Ed. 50, 1083910842 (2011).
NATURE COMMUNICATIONS | 5:4576 | DOI: 10.1038/ncomms5576 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications 9
& 2014 Macmillan Publishers Limited. All rights reserved.
ARTICLE NATURE COMMUNICATIONS | DOI: 10.1038/ncomms5576
27. Paton, K. R. et al. Scalable production of large quantities of defect-free few-layer graphene by shear exfoliation in liquids. Nat. Mater. 13, 624630 (2014).
28. Wang, J. Z. et al. Development of MoS2-CNT composite thin lm from layered MoS2 for lithium batteries. Adv. Energy Mater. 3, 798805 (2013).
29. Smith, R. J. et al. Large-scale exfoliation of inorganic layered compounds in aqueous surfactant solutions. Adv. Mater. 23, 39443948 (2011).
30. Cunningham, G. et al. Photoconductivity of solution-processed MoS2 lms.J. Mater. Chem. C 1, 68996904 (2013).31. May, P., Khan, U. & Coleman, J. N. Reinforcement of metal with liquid-exfoliated inorganic nano-platelets. Appl. Phys. Lett. 103, 163106 (2013).
32. May, P., Khan, U., Hughes, J. M. & Coleman, J. N. Role of solubility parameters in understanding the steric stabilization of exfoliated two-dimensional nanosheets by adsorbed polymers. J. Phys. Chem. C 116, 1139311400 (2012).
33. Hanlon, D. et al. Liquid exfoliation of molybdenum trioxide. Chem. Mater. 26, 17511763 (2013).
34. Naguib, M. et al. Two-dimensional transition metal carbides. ACS Nano 6, 13221331 (2012).
35. Xu, Y., Kominami, K., Ishikawa, Y. & Feng, Q. Layered hydroxide nickel benzoates: hydrothermal synthesis, structure characterization, and exfoliation reaction. J. Colloid. Interface. Sci. 386, 107113 (2012).
36. Khan, U. et al. Size selection of dispersed, exfoliated graphene akes by controlled centrifugation. Carbon 50, 470475 (2012).
37. Lotya, M., Rakovich, A., Donegan, J. F. & Coleman, J. N. Measuring the lateral size of liquid-exfoliated nanosheets with dynamic light scattering. Nanotechnology 24, 265703 (2013).
38. Lee, C. et al. Anomalous lattice vibrations of single- and few-layer MoS2. ACS
Nano 4, 26952700 (2010).39. Svedberg, T., Pederson, K. O. & Bauer, J. H. The Ultracentrifuge (Oxford University Press, 1940).
40. Fagan, J. A., Becker, M. L., Chun, J. & Hobbie, E. K. Length fractionation of carbon nanotubes using centrifugation. Adv. Mater. 20, 16091613 (2008).41. Fagan, J. A. et al. Centrifugal length separation of carbon nanotubes. Langmuir 24, 1388013889 (2008).
42. Sun, X., Luo, D., Liu, J. & Evans, D. G. Monodisperse chemically modied graphene obtained by density gradient ultracentrifugal rate separation. ACS Nano 4, 33813389 (2010).
43. Bonaccorso, F., Zerbetto, M., Ferrari, A. C. & Amendola, V. Sorting nanoparticles by centrifugal elds in clean media. J. Phys. Chem. C 117, 1321713229 (2013).
44. Mak, K. F., Lee, C., Hone, J., Shan, J. & Heinz, T. F. Atomically thin MoS2: a new direct-gap semiconductor. Phys. Rev. Lett. 105, 136805 (2010).
45. Zhao, W. J. et al. Evolution of electronic structure in atomically thin sheets of WS2 and WSe2. ACS Nano 7, 791797 (2013).
46. He, G. S., Qin, H. Y. & Zheng, Q. Rayleigh, Mie, and Tyndall scatterings of polystyrene microspheres in water: wavelength, size, and angle dependences.J. Appl. Phys. 105, 023110 (2009).47. Dolui, K., Das Pemmaraju, C. & Sanvito, S. Electric eld effects on armchair MoS2 nanoribbons. ACS Nano 6, 48234834 (2012).
48. Zhang, C., Johnson, A., Hsu, C.-L., Li, L.-J. & Shih, C.-K. Direct imaging of band prole in single layer MoS2 on graphite: quasiparticle energy gap, metallic edge states, and edge band bending. Nano Lett. 14, 24432447 (2014).
49. Yin, X. et al. Edge nonlinear optics on a MoS2 atomic monolayer. Science 344, 488490 (2014).
50. van der Zande, A. M. et al. Grains and grain boundaries in highly crystalline monolayer molybdenum disulphide. Nat. Mater. 12, 554561 (2013).
51. Mak, K. F., Lee, C., Hone, J., Shan, J. & Heinz, T. F. Atomically thin MoS2. a new direct-gap semiconductor. Phys. Rev. Lett. 105, 136805 (2010).
52. Splendiani, A. et al. Emerging photoluminescence in monolayer MoS2. Nano Lett. 10, 12711275 (2010).
53. Li, H. et al. From bulk to monolayer MoS2: evolution of raman scattering. Adv. Funct. Mater. 22, 13851390 (2012).
54. Mao, N., Chen, Y., Liu, D., Zhang, J. & Xie, L. Solvatochromic effect on the photoluminescence of MoS2 monolayers. Small 9, 13121315 (2013).
55. Jaramillo, T. F. et al. Identication of active edge sites for electrochemical H-2 evolution from MoS2 nanocatalysts. Science 317, 100102 (2007).
56. Gutirrez, H. R. et al. Extraordinary room-temperature photoluminescence in triangular WS2 monolayers. Nano Lett. 13, 34473454 (2012).
Acknowledgements
The research leading to these results has received funding from the European Union Seventh Framework Programme under grant agreement n604391 Graphene Flagship. In addition, J.N.C. acknowledges the European Research Council grant SEMANTICS and the SFI grant number 11/PI/1087 for nancial support. C.B. acknowledges the German research foundation DFG (BA 4856/1-1). V.N. and H.C.N. acknowledge ERC 2DNanoCaps, SFI PIYRA and FP7 MoWSeS. N.S. and J.M. acknowledge support from DFG SPP 1459 (MA 4079/7-1) and European Research Council (grant number 259286). G.S.D. and N.C.B. acknowledge SFI for PI_10/IN.1/I3030. N.M. thanks FP7-2010-PPP Green Cars Electrograph (266391).
Author contributions
C.B., N.M., N.C.B., N.S., J.M., G.S.D., D.M. and J.F.D. performed spectroscopy, C.B., R.J.S., H.C.N., A.O., D.H., L.H. and V.N. performed microscopy, P.J.K. and T.H. fabricated and tested devices, C.B. and J.N.C. planned the experiments and wrote the paper.
Additional information
Supplementary Information accompanies this paper at http://www.nature.com/naturecommunications
Web End =http://www.nature.com/ http://www.nature.com/naturecommunications
Web End =naturecommunications
Competing nancial interests: The authors declare no competing nancial interests.
Reprints and permission information is available online at http://www.nature.com/naturecommunications
Web End =http://npg.nature.com/ http://www.nature.com/naturecommunications
Web End =reprintsandpermissions/
How to cite this article: Backes, C. et al. Edge and connement effects allow in situ measurement of size and thickness of liquid-exfoliated nanosheets. Nat. Commun. 5:4576 doi: 10.1038/ncomms5576 (2014).
10 NATURE COMMUNICATIONS | 5:4576 | DOI: 10.1038/ncomms5576 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications
& 2014 Macmillan Publishers Limited. All rights reserved.
You have requested "on-the-fly" machine translation of selected content from our databases. This functionality is provided solely for your convenience and is in no way intended to replace human translation. Show full disclaimer
Neither ProQuest nor its licensors make any representations or warranties with respect to the translations. The translations are automatically generated "AS IS" and "AS AVAILABLE" and are not retained in our systems. PROQUEST AND ITS LICENSORS SPECIFICALLY DISCLAIM ANY AND ALL EXPRESS OR IMPLIED WARRANTIES, INCLUDING WITHOUT LIMITATION, ANY WARRANTIES FOR AVAILABILITY, ACCURACY, TIMELINESS, COMPLETENESS, NON-INFRINGMENT, MERCHANTABILITY OR FITNESS FOR A PARTICULAR PURPOSE. Your use of the translations is subject to all use restrictions contained in your Electronic Products License Agreement and by using the translation functionality you agree to forgo any and all claims against ProQuest or its licensors for your use of the translation functionality and any output derived there from. Hide full disclaimer
Copyright Nature Publishing Group Aug 2014
Abstract
Two-dimensional nanomaterials such as MoS2 are of great interest both because of their novel physical properties and their applications potential. Liquid exfoliation, an important production method, is limited by our inability to quickly and easily measure nanosheet size, thickness or concentration. Here we demonstrate a method to simultaneously determine mean values of these properties from an optical extinction spectrum measured on a liquid dispersion of MoS2 nanosheets. The concentration measurement is based on the size-independence of the low-wavelength extinction coefficient, while the size and thickness measurements rely on the effect of edges and quantum confinement on the optical spectra. The resultant controllability of concentration, size and thickness facilitates the preparation of dispersions with pre-determined properties such as high monolayer-content, leading to first measurement of A-exciton MoS2 luminescence in liquid suspensions. These techniques are general and can be applied to a range of two-dimensional materials including WS2 , MoSe2 and WSe2 .
You have requested "on-the-fly" machine translation of selected content from our databases. This functionality is provided solely for your convenience and is in no way intended to replace human translation. Show full disclaimer
Neither ProQuest nor its licensors make any representations or warranties with respect to the translations. The translations are automatically generated "AS IS" and "AS AVAILABLE" and are not retained in our systems. PROQUEST AND ITS LICENSORS SPECIFICALLY DISCLAIM ANY AND ALL EXPRESS OR IMPLIED WARRANTIES, INCLUDING WITHOUT LIMITATION, ANY WARRANTIES FOR AVAILABILITY, ACCURACY, TIMELINESS, COMPLETENESS, NON-INFRINGMENT, MERCHANTABILITY OR FITNESS FOR A PARTICULAR PURPOSE. Your use of the translations is subject to all use restrictions contained in your Electronic Products License Agreement and by using the translation functionality you agree to forgo any and all claims against ProQuest or its licensors for your use of the translation functionality and any output derived there from. Hide full disclaimer