1. Introduction
Mg alloys are the lightest metallic structural materials with superior properties, such as excellent castability, good damping capacity, and high specific strength, making them ideal light-weight materials for applications in many industrial fields including automobiles and rail traffic [1,2,3,4,5]. It has been reported that every weight reduction of 100 Kg of a vehicle reduces the fuel consumption by 0.3–0.4 L/100 km [6]. Replacing the steel and Al alloys in vehicles and trains by Mg alloys can significantly reduce the consumption of energy and the emission of CO2, contributing to the alleviation of the energy crisis and global warming. However, the strength of Mg alloys is commonly lower than that required for application as structural materials. The addition of rare earth (RE) elements enhances the mechanical performance of Mg alloys, but substantially boosts the costs, restricting their application. Thus, it is very important to develop high-performance RE-free Mg alloys.
Mg-Sn alloys are deemed promising RE-free Mg alloys because they are similar to RE-containing Mg alloys in two aspects [7]. Firstly, the solubility of Sn in Mg is very high at high temperatures (3.35 at.% at 561 °C), and it reduces to a negligible value at room temperature, making Mg-Sn alloys age-hardenable [8,9,10,11,12]. Secondly, the intermetallic Mg2Sn phase in the Mg-Sn alloys possesses a very high melting temperature of 770 °C [8,9,13]. However, the mechanical performance of the as-cast Mg-Sn alloys is inferior. Thermomechanical processing has been employed to improve the mechanical performance of Mg-Sn alloys [8,14,15,16,17]. Hot extruded Mg-Sn alloys exhibit superior strength compared to their as-cast counterparts [14,15,18]. The strength enhancement is mainly attributed to grain refinement strengthening and precipitation strengthening. As Sn content increases from 1% to 7% (in wt.% unless otherwise noted), the YS and UTS of hot extruded Mg-Sn alloys increase, while EL decreases [18]. Similar results were reported by Cheng et al., in their study on the mechanical properties of hot extruded Mg-(6, 8, 10)Sn alloys [15]. Zhao et al., reported that YS, UTS, and EL increase as the Sn addition increases from 1.3% to 4.7% [19].
Note that previous studies on the hot working of Mg-Sn alloys are mainly focused on hot extrusion and rare attention has been paid to hot rolling. Due to the hexagonal close-packed (HCP) structure, the plasticity of the as-cast Mg alloys is poor [20]. When hot extruded, the Mg-Sn alloys are under a triaxial compressive stress state, which is conducive to improving workability [21]. In contrast, the Mg-Sn alloys are mainly under uniaxial compressive stress state during hot rolling and the workability is relatively poor. Therefore, the hot rolling of Mg-Sn alloys has rarely been reported. Hot rolling is a very efficient and cost-effective technique to fabricate Mg alloy plates with good performance [22,23]. It has been reported that hot rolling can effectively refine the microstructure and thus improve the mechanical performance of Mg alloys [22,24,25,26,27,28,29]. In this work, the effect of hot rolling on the microstructure and mechanical performance of a Mg-5Sn alloy was investigated. The results of this study may provide useful guidance for developing high-performance Mg alloys.
2. Materials and Methods
The raw materials for the fabrication of Mg-5Sn alloy are pure Mg (99.9%) and pure Sn (99.99%) ingots. They were melted in a zinc oxide-coated graphite crucible using an electric resistance furnace. Subsequently, the melt was cast in a zinc oxide-coated steel mold (with a dimension of 200 × 50 × 50 mm3) which was pre-heated to 300 °C. The melting and casting processes were conducted under the protective atmosphere of CO2 (99% in volume) and SF6 (1% in volume). Then, the as-cast alloy was machined into small pieces with a dimension of 19.5 × 42 × 3.5 mm3 through wire electrical discharge machining. Some of the small samples were solid-solution treated at 480 °C for 12 h, which were then hot rolled at 380 °C for three different reductions of 30%, 50%, and 70%, respectively. The samples hot rolled for 30%, 50%, and 70% were denoted as the R30 alloy, R50 alloy, and R70 alloy, respectively. The rolling reduction per pass is 10%.
A CMT5105 electronic universal testing machine was used to perform room temperature tensile tests. The loading rate is 0.5 mm/s and tensile test samples are dog-bone shaped, having a gage length of 7 mm. To obtain reliable results, three specimens were tested for each state. Tensile loading was applied along the rolling direction (RD) for the hot rolled samples. The microstructures were characterized by a ZEISS G300 scanning electron microscopy (SEM, Zeiss, Oberkochen, Germany) equipped with an energy dispersive spectroscopy (EDS) and an electron backscatter diffractions system (EBSD). Channel 5 software was employed to post-process the EBSD data. All of the EBSD results shown in this paper were obtained through using this software. The samples for microstructure characterization were prepared according to the procedure given in ref [30]. The microstructure observations were conducted on the cross-section perpendicular to the normal direction (ND). A schematic diagram of the processing route used in this work is shown in Figure 1.
3. Results
3.1. Microstructures
Figure 2 shows the SEM images of the as-cast and solid-solution treated Mg-5Sn alloys. Note that the as-cast Mg-5Sn alloy contains α-Mg matrix and intermetallic particles. According to previous studies [9,31,32,33], the intermetallic particles in the Mg-Sn binary alloys are Mg2Sn phase. The EDS analysis shown in Figure 2b confirms that the intermetallic compounds are Mg2Sn phase. α-Mg dendrites are very coarse with an arm spacing ranging from tens of microns to hundreds of microns. The Mg2Sn intermetallic compounds exhibit plate-like morphology. They are very coarse, and some of them have a length larger than 100 μm. The solid-solution treatment dissolved most of the Mg2Sn particles. Few of the Mg2Sn particles can still be observed near the grain boundaries, but their size is much smaller than that in the as-cast alloy, consistent with the previous studies [14,15].
Figure 3 shows the inverse pole figure (IPF) maps of the hot rolled alloys, along with the corresponding grain size distribution. The grains are colored by their crystallographic orientations with red, blue, and green denoting [0001], , and directions, respectively. The hot rolled alloys possess much finer grains than the as-cast alloy. The grain size decreases from 13.52 μm to 11.65 μm and further to 4.71 μm, with the increase of the rolling reduction from 30% to 50% and further to 70%. The grain refinement is attributed to dynamic recrystallization (DRX) during hot rolling. As rolling reduction increases, the plastic deformation becomes severer, and the strain inside the alloy becomes larger. The strain distribution within the alloy can be estimated by kernel average misorientation (KAM) maps, because the severely deformed regions usually exhibit higher dislocation densities and thus larger KAM values [34,35]. The KAM images of the hot rolled alloys are shown in Figure 4. Noticeably, the average KAM value increases continuously with the increase of the rolling reduction from 30% to 70%, indicating the increase in dislocation density with the increase in rolling reduction. A higher dislocation density provides a larger driving force for DRX [36]. Increasing the rolling reduction can promote DRX and grain refinement [25]. Therefore, as the rolling reduction increases from 30% to 70%, the grain size decreases continuously.
The SEM images of the hot rolled Mg-5Sn alloys are exhibited in Figure 5. Numerous fine particles can be observed in all three alloys. These fine particles are Mg2Sn precipitates formed during hot rolling through dynamic precipitation. The previous studies [15,37,38] demonstrate that plastic deformation can induce the dynamic precipitation of Mg2Sn phase. Our observation is consistent with previous studies [15,37,38]. Moreover, some coarse undissolved Mg2Sn particles exist in the alloys. The morphology of the undissolved Mg2Sn particles changes from plate-like in the as-cast alloy to “blocky” and their size is much smaller. Some of the undissolved Mg2Sn particles were fragmentized during hot rolling, as shown in Figure 5h.
It can be noted from Figure 5 that the size and area fraction of Mg2Sn particles are affected by rolling reduction. The average size and area fraction of Mg2Sn particles in the R30 alloy are 2.10 μm and 5.53%, respectively. As the rolling reduction increases to 50%, the average size of Mg2Sn particles increases slightly to 2.30 μm, but their area fraction rises to 13.48% (Figure 5f). With the further increase of the rolling reduction to 70%, the average size and area fraction of Mg2Sn particles increase to 3.30 μm and 14.7%, respectively. The formation of the Mg2Sn precipitates is due to dynamic precipitation during thermomechanical processing, as reported in previous studies [15,37,38]. The dislocations formed during plastic deformation can not only provide nucleation sites for the dynamic precipitation of the Mg2Sn phase, but also increase the diffusion rate of the Sn atoms [15,37]. When the rolling reduction is 30%, the dislocation density is relatively low (Figure 4d) and therefore the area fraction of Mg2Sn precipitates is relatively low. As the rolling reduction increases to 50%, more dislocations are accumulated in the alloy (Figure 4e), providing more nucleation sites for Mg2Sn phase. In addition, the pre-existing Mg2Sn precipitates may act as nucleation sites. Consequently, the area fraction of Mg2Sn particles for R50 alloy rises to 13.48% and their average size increases slightly. A further increase of the rolling reduction to 70% generates more dislocations (Figure 4f) and thus leads to the further increase in the average size and area fraction of Mg2Sn particles.
3.2. Mechanical Properties
Engineering the stress–strain curves of the as-cast and hot rolled alloys are presented in Figure 6. Their YS, UTS, and EL are presented in Table 1. It can be noted that the strengths of hot rolled alloys are much higher than that of the as-cast alloy. In addition, YS and UTS of the hot rolled alloys increase continuously with increasing rolling reduction, whereas the EL of the alloys shows an opposite trend. The R70 alloy has the highest UTS of 310 MPa, but the lowest EL of 8.4%. The R30 alloy possesses a much better ductility than the as-cast alloy while the R50 and R70 alloys have a ductility similar to that of the as-cast alloy. The mechanical performance of the R70 alloy is compared with that of the recently developed hot rolled Mg-Sn alloys, as shown in Figure 7. It can be noted that the R70 alloy exhibits good comprehensive mechanical properties.
The enhanced strength of the hot rolled alloys can be ascribed to precipitation strengthening, grain refinement strengthening, and dislocation strengthening. The strengthening effect of fine and dense precipitates is stronger than that of coarse and sparse particles [39]. The finer grains can exert a stronger strengthening effect than coarse grains [40]. Dislocations of a higher density results in a stronger dislocation strengthening [41]. The coarse grains and Mg2Sn phase in the as-cast alloy (Figure 2) are less effective in strengthening the alloy compared to the relatively fine grains and Mg2Sn precipitates in the hot rolled alloys (Figure 3 and Figure 5). In addition, the plastic deformation induces the accumulation of dislocations in the hot rolled alloys, as indicated by the KAM maps shown in Figure 4. Therefore, the hot rolled alloys have a much higher strength than the as-cast alloy. As the rolling reduction increases from 30% to 70%, the grain size decreases while the area fraction of Mg2Sn particles and dislocation density (as implied by the KAM value) increase continuously. Therefore, the strengths of the hot rolled alloys exhibit a rising trend with increasing rolling reduction.
Figure 7Mechanical performance comparison between the R70 alloy developed in this work and recently developed hot rolled Mg-Sn alloys [14,15,17,18,19,42,43,44,45,46,47,48].
[Figure omitted. See PDF]
According to the Hall–Petch relation [49], the yield strength is related to grain size d by:
(1)
where is lattice friction stress; [50]; and k is the Hall–Petch slope, [8]. Substituting the values of the grain size into Equation (1), we can obtain the for as-cast and hot rolled alloys. Subtracting the for the as-cast alloy from that for the hot rolled alloys, we can obtain the strength enhancement induced by grain refinement strengthening . for the R30, R50, and R70 alloys were calculated to be 48.1, 54.2, and 100.9 MPa, respectively.The strength increment caused by dislocation strengthening can be estimated by the Bailey–Hirsch equation [51]:
(2)
where M is the Taylor factor (M = 2.1 [52]); is the Taylor constant ( = 0.2 [50]); G is the shear modulus of Mg (G = 16.6 GPa [53]); b is the Burgers vector for basal slip of Mg (b = 0.321 nm [53]); and denotes the dislocation density of the alloy. can be evaluated by [54]:(3)
where represents the local misorientation angle obtained from the EBSD KAM maps (Figure 4) and u is the EBSD step size. u is 0.6 μm for the R30 and R50 alloys and 0.3 μm for R70 alloy. Combining Equations (2) and (3), the for the R30, R50, and R70 alloys can be obtained as 25.7, 27.2, and 43.6 MPa, respectively.Strength enhancement arising from precipitation strengthening can be calculated by the Orowan–Ashby equation [55]:
(4)
where is the interparticle distance and is the average particle size. for the R30, R50, and R70 alloys were estimated to be 5.5, 9.7, and 18.6 MPa, respectively.The total strength increment induced by the three strengthening mechanisms can be calculated by:
(5)
for the R30, R50, and R70 alloys were estimated to be 79.3, 90.9, and 163.2 MPa, respectively. As can be seen from Table 1, the YS of the R30, R50, and R70 alloys exceed that of the as-cast alloy by 74, 92, and 160 MPa, respectively. The calculated strength enhancement is in good agreement with experimental results. It can be noted from comparing values of , , and that grain refinement strengthening is the dominant strengthening mechanism, followed by dislocation strengthening.
The fracture surfaces of the as-cast and hot rolled alloys are displayed in Figure 8. As-cast alloy exhibits the typical characteristics of brittle fracture, with many cleavage steps on the fracture surfaces. Dimples can be observed on the fracture surfaces of the R30 and R50 alloys, exhibiting to some extent the feature of a micro-void coalescence fracture. Therefore, the ductility of the R30 and R50 alloys are better than the as-cast alloy. As the rolling reduction increases to 70%, the cleavage steps and river patterns appear again, indicating the drop in ductility. The trend of ductility with the variation of rolling reduction deduced from fracture surfaces is consistent with that observed from the engineering stress–strain curves shown in Figure 6. The Mg2Sn phase is hard and brittle while the Mg matrix is relatively soft. Due to the deformation incompatibility, the stress concentration is induced at the interface between the coarse Mg2Sn particles and Mg matrix. When the stress concentration reaches a critical level, the interfacial cracks nucleate and propagate, leading the fracture of Mg-5Sn alloy [15,44,56].
The ductility of the metallic materials is also related to precipitates, grain size, and dislocation density. The grain boundaries, precipitates, and high-density dislocations can act as dislocation barriers and block dislocation movements, leading to dislocation accumulation and promoting stress concentration [57,58,59,60]. Therefore, fine grains, high-density precipitates, and high-density dislocations may generally have a negative influence on ductility. With the increase of rolling reduction from 30% to 70%, the area fraction of the Mg2Sn particles and dislocation density increase, and meanwhile the grain size decreases. Therefore, the EL of hot rolled Mg-Sn alloys shows a decreasing trend with increasing rolling reduction. As-cast alloy has poorer ductility compared to the R30 alloy, due to the presence of the coarse Mg2Sn phase which may act as crack nucleation sites.
4. Conclusions
The microstructure evolution and mechanical properties of a Mg-5Sn alloy which was hot rolled at three different rolling reductions (30%, 50%, and 70%) were investigated in this work. The grain size of hot rolled alloys decreases from 13.5 to 4.7 μm as rolling reduction increases from 30% to 70%. In contrast, the area fraction of the Mg2Sn particles and dislocation density rise with the increase in rolling reduction. Consequently, the strengths of the alloys exhibit an increasing trend with increasing rolling reduction, whereas the EL of the alloys shows a decreasing trend. Specifically, the UTS of the hot rolled alloys increases from 213 to 310 MPa while the EL of the hot rolled alloys decreases from 14.1% to 8.4% with the increase of rolling reduction from 30% to 70%. Strength enhancement is mainly ascribed to precipitation strengthening, grain refinement strengthening, and dislocation strengthening. Hot rolled alloys possess much better comprehensive mechanical properties than the as-cast alloy.
Conceptualization, X.Z., H.L. and Z.H.; methodology, X.Z., H.L. and Z.H.; investigation, X.Z., C.S. and P.Z.; data curation, C.S.; writing—original draft preparation, X.Z.; writing—review and editing, H.L. and Z.H.; supervision, Z.H. All authors have read and agreed to the published version of the manuscript.
The authors declare no conflict of interest.
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.
Figure 2. SEM images of (a,b) as-cast Mg-5Sn alloy; and (c,d) solid solution treated Mg-5Sn alloy. The inset in (b) is the result of EDS analysis of area A.
Figure 3. IPF maps of (a) R30 alloy; (b) R50 alloy; and (c) R70 alloy. Statics of grains in (d) R30 alloy; (e) R50 alloy; and (f) R70 alloy.
Figure 4. KAM maps of (a) R30 alloy; (b) R50 alloy; and (c) R70 alloy. Statics of KAM angle in (d) R30 alloy; (e) R50 alloy; and (f) R70 alloy.
Figure 5. SEM images of (a,b) R30 alloy; (d,e) R50 alloy; and (g,h) R70 alloy. Statics of Mg2Sn phase in (c) R30 alloy; (f) R50 alloy; and (i) R70 alloy.
Figure 6. Engineering stress–engineering strain curves of as-cast and hot rolled alloys.
Figure 8. Fracture surfaces of (a,b) as-cast alloy; (c,d) R30 alloy; (e,f) R50 alloy; and (g,h) R70 alloy.
YS, UTS, and EL of as-cast and hot rolled Mg-5Sn alloys.
Alloys | YS (MPa) | UTS (MPa) | EL (%) |
---|---|---|---|
As-cast alloy | 31 | 133 | 9.8 |
R30 alloy | 105 | 213 | 14.1 |
R50 alloy | 123 | 252 | 10.5 |
R70 alloy | 191 | 310 | 8.4 |
References
1. Bovand, D.; Abdollah-Pour, H.; Mirzaee, O.; Bagherifard, S. Dry sliding wear and corrosion performance of Mg-Sn-Ti alloys produced by casting and extrusion. Materials; 2022; 15, 3533. [DOI: https://dx.doi.org/10.3390/ma15103533] [PubMed: https://www.ncbi.nlm.nih.gov/pubmed/35629559]
2. Xu, H.; Li, Y.; Wu, L.; Jiang, F.; Fu, D.; Teng, J.; Zhang, H. Effect of heat treatments on the corrosion resistance of a high strength Mg-Gd-Y-Zn-Zr alloy. Materials; 2022; 15, 2813. [DOI: https://dx.doi.org/10.3390/ma15082813] [PubMed: https://www.ncbi.nlm.nih.gov/pubmed/35454505]
3. Xu, T.; Yang, Y.; Peng, X.; Song, J.; Pan, F. Overview of advancement and development trend on magnesium alloy. J. Magnes. Alloy.; 2019; 7, pp. 536-544. [DOI: https://dx.doi.org/10.1016/j.jma.2019.08.001]
4. Zuo, J.; Zhang, M.; Nakata, T.; Wang, G.; Li, D.; Shi, H.; Xu, C.; Wang, X.; Li, W.; Fan, G. et al. Effect of Al addition on grain refinement and phase transformation of the Mg-Gd-Y-Zn-Mn alloy containing LPSO phase. Materials; 2022; 15, 1632. [DOI: https://dx.doi.org/10.3390/ma15051632]
5. Zhuo, X.R.; Ma, A. Molecular dynamics-based cohesive zone model for Mg/Mg17Al12 interface. Metals; 2020; 10, 836. [DOI: https://dx.doi.org/10.3390/met10060836]
6. Cheah, L.; Heywood, J. Meeting U.S. passenger vehicle fuel economy standards in 2016 and beyond. Energy Policy; 2011; 39, pp. 454-466. [DOI: https://dx.doi.org/10.1016/j.enpol.2010.10.027]
7. Fu, H.; Guo, J.; Wu, W.; Liu, B.; Peng, Q. High pressure aging synthesis of a hexagonal Mg2Sn strengthening precipitate in Mg-Sn alloys. Mater. Lett.; 2015; 157, pp. 172-175. [DOI: https://dx.doi.org/10.1016/j.matlet.2015.05.087]
8. Cheng, W.L.; Tian, Q.W.; Yu, H.; Zhang, H.; You, B.S. Strengthening mechanisms of indirect-extruded Mg–Sn based alloys at room temperature. J. Magnes. Alloy.; 2014; 2, pp. 299-304. [DOI: https://dx.doi.org/10.1016/j.jma.2014.11.003]
9. Liu, H.; Chen, Y.; Tang, Y.; Wei, S.; Niu, G. The microstructure, tensile properties, and creep behavior of as-cast Mg–(1–10)% Sn alloys. J. Alloy. Compd.; 2007; 440, pp. 122-126. [DOI: https://dx.doi.org/10.1016/j.jallcom.2006.09.024]
10. Liu, C.Q.; Chen, H.W.; Liu, H.; Zhao, X.J.; Nie, J.F. Metastable precipitate phases in Mg–9.8 wt%Sn alloy. Acta Mater.; 2018; 144, pp. 590-600. [DOI: https://dx.doi.org/10.1016/j.actamat.2017.10.023]
11. Wei, S.-H.; Chen, Y.-G.; Tang, Y.-B.; Liu, M.; Xiao, S.-F.; Zhang, X.-P.; Zhao, Y.-H. Compressive creep behavior of Mg-Sn binary alloy. Trans. Nonferrous Met. Soc. China; 2008; 18, pp. S214-S217. [DOI: https://dx.doi.org/10.1016/S1003-6326(10)60205-1]
12. Wei, S.; Chen, Y.; Tang, Y.; Liu, H.; Mao, S.; Niu, G.; Zhang, X.; Zhao, Y. Compressive creep behavior of as-cast and aging-treated Mg-5 wt% Sn alloys. Mater. Sci. Eng. A-Struct. Mater. Prop. Microstruct. Process.; 2008; 492, pp. 20-23. [DOI: https://dx.doi.org/10.1016/j.msea.2008.05.006]
13. Cheng, W.; Bai, Y.; Wang, L.; Wang, H.; Bian, L.; Yu, H. Strengthening effect of extruded Mg-8Sn-2Zn-2Al alloy: Influence of micro and nano-size Mg2Sn precipitates. Materials; 2017; 10, 822. [DOI: https://dx.doi.org/10.3390/ma10070822]
14. Chen, D.; Ren, Y.-P.; Guo, Y.; Pei, W.-L.; Zhao, H.-D.; Qin, G.-W. Microstructures and tensile properties of as-extruded Mg-Sn binary alloys. Trans. Nonferrous Met. Soc. China; 2010; 20, pp. 1321-1325. [DOI: https://dx.doi.org/10.1016/S1003-6326(09)60298-3]
15. Cheng, W.L.; Park, S.S.; You, B.S.; Koo, B.H. Microstructure and mechanical properties of binary Mg-Sn alloys subjected to indirect extrusion. Mater. Sci. Eng. A-Struct. Mater. Prop. Microstruct. Process.; 2010; 527, pp. 4650-4653. [DOI: https://dx.doi.org/10.1016/j.msea.2010.03.031]
16. Li, W. Compression yield behavior and corresponding microstructure characterization of Mg-1.5Sn (at.%) alloys. Mater. Res. Express; 2021; 8, 106502. [DOI: https://dx.doi.org/10.1088/2053-1591/ac29a4]
17. Wan, Y.J.; Zeng, Y.; Zeng, Q.; Song, B.; Huang, X.F.; Qian, X.Y.; Jiang, B. Simultaneously improved strength and toughness of a Mg-Sn alloy through abundant prismatic lath-shaped precipitates. Mater. Sci. Eng. A-Struct. Mater. Prop. Microstruct. Process.; 2021; 811, 141087. [DOI: https://dx.doi.org/10.1016/j.msea.2021.141087]
18. Zhao, C.; Pan, F.; Zhao, S.; Pan, H.; Song, K.; Tang, A. Preparation and characterization of as-extruded Mg-Sn alloys for orthopedic applications. Mater. Des.; 2015; 70, pp. 60-67. [DOI: https://dx.doi.org/10.1016/j.matdes.2014.12.041]
19. Zhao, C.; Chen, X.; Pan, F.; Gao, S.; Zhao, D.; Liu, X. Effect of Sn content on strain hardening behavior of as-extruded Mg-Sn alloys. Mater. Sci. Eng. A-Struct. Mater. Prop. Microstruct. Process.; 2018; 713, pp. 244-252. [DOI: https://dx.doi.org/10.1016/j.msea.2017.12.074]
20. Prasad, S.V.S.; Prasad, S.B.; Verma, K.; Mishra, R.K.; Kumar, V.; Singh, S. The role and significance of Magnesium in modern day research-A review. J. Magnes. Alloy.; 2022; 10, pp. 1-61. [DOI: https://dx.doi.org/10.1016/j.jma.2021.05.012]
21. Wang, X.J.; Nie, K.B.; Hu, X.S.; Wang, Y.Q.; Sa, X.J.; Wu, K. Effect of extrusion temperatures on microstructure and mechanical properties of SiCp/Mg-Zn-Ca composite. J. Alloy. Compd.; 2012; 532, pp. 78-85. [DOI: https://dx.doi.org/10.1016/j.jallcom.2012.04.023]
22. Ma, C.-Y.; Xia, N.; Wang, C.; Li, M.-X.; Hua, Z.-M.; Ren, M.-W.; Wang, H.-Y. A novel Mg-5Al-2Zn-2Sn alloy with high strength-ductility synergy fabricated via simple hot rolling and annealing treatment. J. Alloy. Compd.; 2021; 869, 159308. [DOI: https://dx.doi.org/10.1016/j.jallcom.2021.159308]
23. Nakata, T.; Xu, C.; Ohashi, H.; Yoshida, Y.; Yoshida, K.; Kamado, S. New Mg-Al based alloy sheet with good room-temperature stretch formability and tensile properties. Scr. Mater.; 2020; 180, pp. 16-22. [DOI: https://dx.doi.org/10.1016/j.scriptamat.2020.01.015]
24. Guo, F.; Zhang, D.; Wu, H.; Jiang, L.; Pan, F. The role of Al content on deformation behavior and related texture evolution during hot rolling of Mg-Al-Zn alloys. J. Alloy. Compd.; 2017; 695, pp. 396-403. [DOI: https://dx.doi.org/10.1016/j.jallcom.2016.10.222]
25. Guo, F.; Zhang, D.; Yang, X.; Jiang, L.; Chai, S.; Pan, F. Effect of rolling speed on microstructure and mechanical properties of AZ31 Mg alloys rolled with a wide thickness reduction range. Mater. Sci. Eng. A-Struct. Mater. Prop. Microstruct. Process.; 2014; 619, pp. 66-72. [DOI: https://dx.doi.org/10.1016/j.msea.2014.09.024]
26. Jin, L.; Dong, J.; Wang, R.; Peng, L.M. Effects of hot rolling processing on microstructures and mechanical properties of Mg-3%Al-1%Zn alloy sheet. Mater. Sci. Eng. A-Struct. Mater. Prop. Microstruct. Process.; 2010; 527, pp. 1970-1974. [DOI: https://dx.doi.org/10.1016/j.msea.2009.11.047]
27. Wang, J.; Dong, H.; Wang, L.; Wu, Y.; Wang, L. Effect of hot rolling on the microstructure and mechanical properties of Mg-5Al-0.3Mn-2Nd alloy. J. Alloy. Compd.; 2010; 507, pp. 178-183. [DOI: https://dx.doi.org/10.1016/j.jallcom.2010.07.149]
28. Wu, S.; Zhang, J.; Zhang, Z.; Xu, C.; Nie, K.; Niu, X. A high strength and good ductility Mg-Y-NI-TI alloy with long period stacking ordered structure processed by hot rolling and aging treatment. Mater. Sci. Eng. A-Struct. Mater. Prop. Microstruct. Process.; 2015; 648, pp. 134-139. [DOI: https://dx.doi.org/10.1016/j.msea.2015.09.057]
29. Xu, S.; Zhu, C.; Lin, Z.; Jin, C.; Kamado, S.; Oh-ishi, K.; Qin, Y. Dynamic microstructure evolution and mechanical properties of dilute Mg-Al-Ca-Mn alloy during hot rolling. J. Mater. Sci. Technol.; 2022; 129, pp. 1-14. [DOI: https://dx.doi.org/10.1016/j.jmst.2022.03.029]
30. Liu, H.; Sun, C.; Wang, C.; Li, Y.; Bai, J.; Xue, F.; Ma, A.; Jiang, J. Improving toughness of a Mg2Ca-containing Mg-Al-Ca-Mn alloy via refinement and uniform dispersion of Mg2Ca particles. J. Mater. Sci. Technol.; 2020; 59, pp. 61-71. [DOI: https://dx.doi.org/10.1016/j.jmst.2020.02.092]
31. Poddar, P.; Bagui, S.; Ashok, K.; Murugesan, A.P. Experimental investigation on microstructure and mechanical properties of gravity-die-cast magnesium alloys. J. Alloy. Compd.; 2017; 695, pp. 895-908. [DOI: https://dx.doi.org/10.1016/j.jallcom.2016.10.193]
32. Nayyeri, G.; Mahmudi, R. Enhanced creep properties of a cast Mg-5Sn alloy subjected to aging-treatment. Mater. Sci. Eng. A-Struct. Mater. Prop. Microstruct. Process.; 2010; 527, pp. 4613-4618. [DOI: https://dx.doi.org/10.1016/j.msea.2010.04.015]
33. Zhuo, X.; Shao, C.; Zhang, P.; Hu, Z.; Liu, H. Effect of equal channel angular pressing on the microstructure and mechanical properties of an Mg–5Sn Alloy. Metals; 2022; 12, 1341. [DOI: https://dx.doi.org/10.3390/met12081341]
34. Rui, S.-S.; Han, Q.-N.; Wang, X.; Li, S.; Ma, X.; Su, Y.; Cai, Z.; Du, D.; Shi, H.-J. Correlations between two EBSD-based metrics Kernel Average Misorientation and Image Quality on indicating dislocations of near-failure low alloy steels induced by tensile and cyclic deformations. Mater. Today Commun.; 2021; 27, 102445. [DOI: https://dx.doi.org/10.1016/j.mtcomm.2021.102445]
35. Kamaya, M.; Sakakibara, Y.; Yoda, R.; Suzuki, S.; Morita, H.; Kobayashi, D.; Yamagiwa, K.; Nishioka, T.; Maekawa, Y.; Tanakamaru, T. et al. A round robin EBSD measurement for quantitative assessment of small plastic strain. Mater. Charact.; 2020; 170, 110662. [DOI: https://dx.doi.org/10.1016/j.matchar.2020.110662]
36. Huang, K.; Loge, R.E. A review of dynamic recrystallization phenomena in metallic materials. Mater. Des.; 2016; 111, pp. 548-574. [DOI: https://dx.doi.org/10.1016/j.matdes.2016.09.012]
37. Sasaki, T.T.; Yamamoto, K.; Honma, T.; Kamado, S.; Hono, K. A high-strength Mg-Sn-Zn-Al alloy extruded at low temperature. Scr. Mater.; 2008; 59, pp. 1111-1114. [DOI: https://dx.doi.org/10.1016/j.scriptamat.2008.07.042]
38. Kim, B.; Baek, S.-M.; Jeong, H.Y.; Lee, J.G.; Park, S.S. Grain refinement and reduced yield asymmetry of extruded Mg-5Sn-1Zn alloy by Al addition. J. Alloy. Compd.; 2016; 660, pp. 304-309. [DOI: https://dx.doi.org/10.1016/j.jallcom.2015.11.133]
39. Zhuo, X.; Wu, Y.; Ju, J.; Liu, H.; Jiang, J.; Hu, Z.; Bai, J.; Xue, F. Recent progress of novel biodegradable zinc alloys: From the perspective of strengthening and toughening. J. Mater. Res. Technol-JMRT; 2022; 17, pp. 244-269. [DOI: https://dx.doi.org/10.1016/j.jmrt.2022.01.004]
40. Hansen, N. Hall-Petch relation and boundary strengthening. Scr. Mater.; 2004; 51, pp. 801-806. [DOI: https://dx.doi.org/10.1016/j.scriptamat.2004.06.002]
41. Zhang, X.; Hansen, N.; Gao, Y.; Huang, X. Hall-Petch and dislocation strengthening in graded nanostructured steel. Acta Mater.; 2012; 60, pp. 5933-5943. [DOI: https://dx.doi.org/10.1016/j.actamat.2012.07.037]
42. El Mahallawy, N.; Diaa, A.A.; Akdesir, M.; Palkowski, H. Effect of Zn addition on the microstructure and mechanical properties of cast, rolled and extruded Mg-6Sn-xZn alloys. Mater. Sci. Eng. A-Struct. Mater. Prop. Microstruct. Process.; 2017; 680, pp. 47-53. [DOI: https://dx.doi.org/10.1016/j.msea.2016.10.075]
43. Pan, H.; Qin, G.; Xu, M.; Fu, H.; Ren, Y.; Pan, F.; Gao, Z.; Zhao, C.; Yang, Q.; She, J. et al. Enhancing mechanical properties of Mg-Sn alloys by combining addition of Ca and Zn. Mater. Des.; 2015; 83, pp. 736-744. [DOI: https://dx.doi.org/10.1016/j.matdes.2015.06.032]
44. Jayalakshmi, S.; Sankaranarayanan, S.; Koh, S.P.X.; Gupta, M. Effect of Ag and Cu trace additions on the microstructural evolution and mechanical properties of Mg-5Sn alloy. J. Alloy. Compd.; 2013; 565, pp. 56-65. [DOI: https://dx.doi.org/10.1016/j.jallcom.2013.02.186]
45. Qian, X.Y.; Zeng, Y.; Jiang, B.; Yang, Q.R.; Wan, Y.J.; Quan, G.F.; Pan, F.S. Grain refinement mechanism and improved mechanical properties in Mg-Sn alloy with trace Y addition. J. Alloy. Compd.; 2020; 820, 153122. [DOI: https://dx.doi.org/10.1016/j.jallcom.2019.153122]
46. Chai, Y.; Jiang, B.; Song, J.; Liu, B.; Huang, G.; Zhang, D.; Pan, F. Effects of Zn and Ca addition on microstructure and mechanical properties of as-extruded Mg-1.0Sn alloy sheet. Mater. Sci. Eng. A-Struct. Mater. Prop. Microstruct. Process.; 2019; 746, pp. 82-93. [DOI: https://dx.doi.org/10.1016/j.msea.2019.01.028]
47. Liao, H.; Kim, J.; Liu, T.; Tang, A.; She, J.; Peng, P.; Pan, F. Effects of Mn addition on the microstructures, mechanical properties and work-hardening of Mg-1Sn alloy. Mater. Sci. Eng. A-Struct. Mater. Prop. Microstruct. Process.; 2019; 754, pp. 778-785. [DOI: https://dx.doi.org/10.1016/j.msea.2019.02.021]
48. Zhang, J.; Liu, B.; Jiang, B.; Yang, H.; Zhou, G.; Dai, J.; Pan, F. Role of secondary phase in microstructural stability of as-extruded Mg-Sn-Ca at high temperature. Mater. Sci. Technol.; 2016; 32, pp. 1818-1825. [DOI: https://dx.doi.org/10.1080/02670836.2016.1148218]
49. Yu, H.; Xin, Y.; Wang, M.; Liu, Q. Hall-Petch relationship in Mg alloys: A review. J. Mater. Sci. Technol.; 2018; 34, pp. 248-256. [DOI: https://dx.doi.org/10.1016/j.jmst.2017.07.022]
50. Guan, K.; Yang, Q.; Bu, F.; Qiu, X.; Sun, W.; Zhang, D.; Zheng, T.; Niu, X.; Liu, X.; Meng, J. Microstructures and mechanical properties of a high-strength Mg-3.5Sm-0.6Zn-0.5Zr alloy. Mater. Sci. Eng. A-Struct. Mater. Prop. Microstruct. Process.; 2017; 703, pp. 97-107. [DOI: https://dx.doi.org/10.1016/j.msea.2017.07.058]
51. Bailey, J.; Hirsch, P.J.P.M. The dislocation distribution, flow stress, and stored energy in cold-worked polycrystalline silver. Philos. Mag.; 1960; 5, pp. 485-497. [DOI: https://dx.doi.org/10.1080/14786436008238300]
52. Caceres, C.H.; Lukac, P. Strain hardening behaviour and the Taylor factor of pure magnesium. Philos. Mag.; 2008; 88, pp. 977-989. [DOI: https://dx.doi.org/10.1080/14786430801968611]
53. Wan, Y.; Tang, B.; Gao, Y.; Tang, L.; Sha, G.; Zhang, B.; Liang, N.; Liu, C.; Jiang, S.; Chen, Z. et al. Bulk nanocrystalline high-strength magnesium alloys prepared via rotary swaging. Acta Mater.; 2020; 200, pp. 274-286. [DOI: https://dx.doi.org/10.1016/j.actamat.2020.09.024]
54. Ma, X.; Huang, C.; Moering, J.; Ruppert, M.; Hoeppel, H.W.; Goeken, M.; Narayan, J.; Zhu, Y. Mechanical properties of copper/bronze laminates: Role of interfaces. Acta Mater.; 2016; 116, pp. 43-52. [DOI: https://dx.doi.org/10.1016/j.actamat.2016.06.023]
55. Sun, W.T.; Qiao, X.G.; Zheng, M.Y.; Xu, C.; Kamado, S.; Zhao, X.J.; Chen, H.W.; Gao, N.; Starink, M.J. Altered ageing behaviour of a nanostructured Mg-8.2Gd-3.8Y-1.0Zn-0.4Zr alloy processed by high pressure torsion. Acta Mater.; 2018; 151, pp. 260-270. [DOI: https://dx.doi.org/10.1016/j.actamat.2018.04.003]
56. Huang, S.H. Microstructure and Mechanical Properties of a Ag Micro-Alloyed Mg-5Sn Alloy. J. Mater. Eng. Perform.; 2018; 27, pp. 3199-3205. [DOI: https://dx.doi.org/10.1007/s11665-018-3433-4]
57. Zhang, Z.; Zhang, J.; Xie, J.; Liu, S.; He, Y.; Guan, K.; Wu, R. Developing a low-alloyed fine-grained Mg alloy with high strength-ductility based on dislocation evolution and grain boundary segregation. Scr. Mater.; 2022; 209, 114414. [DOI: https://dx.doi.org/10.1016/j.scriptamat.2021.114414]
58. Zhang, Z.; Zhang, J.-H.; Wang, J.; Li, Z.-H.; Xie, J.-S.; Liu, S.-J.; Guan, K.; Wu, R.-Z. Toward the development of Mg alloys with simultaneously improved strength and ductility by refining grain size via the deformation process. Int. J. Miner. Metall. Mater.; 2021; 28, pp. 30-45. [DOI: https://dx.doi.org/10.1007/s12613-020-2190-1]
59. Wei, X.; Jin, L.; Wang, F.; Li, J.; Ye, N.; Zhang, Z.; Dong, J. High strength and ductility Mg-8Gd-3Y-0.5Zr alloy with bimodal structure and nano-precipitates. J. Mater. Sci. Technol.; 2020; 44, pp. 19-23. [DOI: https://dx.doi.org/10.1016/j.jmst.2019.10.024]
60. Zhuo, X.; Zhang, Q.; Liu, H.; Hu, Z.; Zhang, P.; Jiang, J.; Ma, A.; Wu, Y. Enhanced tensile strength and ductility of an Al-6Si-3Cu alloy processed by room temperature rolling. J. Alloy. Compd.; 2022; 899, 163321. [DOI: https://dx.doi.org/10.1016/j.jallcom.2021.163321]
You have requested "on-the-fly" machine translation of selected content from our databases. This functionality is provided solely for your convenience and is in no way intended to replace human translation. Show full disclaimer
Neither ProQuest nor its licensors make any representations or warranties with respect to the translations. The translations are automatically generated "AS IS" and "AS AVAILABLE" and are not retained in our systems. PROQUEST AND ITS LICENSORS SPECIFICALLY DISCLAIM ANY AND ALL EXPRESS OR IMPLIED WARRANTIES, INCLUDING WITHOUT LIMITATION, ANY WARRANTIES FOR AVAILABILITY, ACCURACY, TIMELINESS, COMPLETENESS, NON-INFRINGMENT, MERCHANTABILITY OR FITNESS FOR A PARTICULAR PURPOSE. Your use of the translations is subject to all use restrictions contained in your Electronic Products License Agreement and by using the translation functionality you agree to forgo any and all claims against ProQuest or its licensors for your use of the translation functionality and any output derived there from. Hide full disclaimer
© 2022 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license (https://creativecommons.org/licenses/by/4.0/). Notwithstanding the ProQuest Terms and Conditions, you may use this content in accordance with the terms of the License.
Abstract
A Mg-5Sn alloy was hot rolled at 380 °C with three different rolling reductions (30%, 50%, and 70%), and its effect on the microstructure and mechanical performance was examined. Grain size decreases, whereas the area fraction of Mg2Sn particles and dislocation density increase with the increase in rolling reduction. Therefore, the yield strength (YS) and ultimate tensile strength (UTS) exhibit an ascending trend, whereas the elongation (EL) shows a descending trend with increasing rolling reduction. The alloy hot rolled for 70% possesses a high strength of 310 MPa and an EL of 8.4%. The strength enhancement is mainly ascribed to precipitation strengthening, grain refinement strengthening, and dislocation strengthening.
You have requested "on-the-fly" machine translation of selected content from our databases. This functionality is provided solely for your convenience and is in no way intended to replace human translation. Show full disclaimer
Neither ProQuest nor its licensors make any representations or warranties with respect to the translations. The translations are automatically generated "AS IS" and "AS AVAILABLE" and are not retained in our systems. PROQUEST AND ITS LICENSORS SPECIFICALLY DISCLAIM ANY AND ALL EXPRESS OR IMPLIED WARRANTIES, INCLUDING WITHOUT LIMITATION, ANY WARRANTIES FOR AVAILABILITY, ACCURACY, TIMELINESS, COMPLETENESS, NON-INFRINGMENT, MERCHANTABILITY OR FITNESS FOR A PARTICULAR PURPOSE. Your use of the translations is subject to all use restrictions contained in your Electronic Products License Agreement and by using the translation functionality you agree to forgo any and all claims against ProQuest or its licensors for your use of the translation functionality and any output derived there from. Hide full disclaimer
Details


1 Nanjing Institute of Agricultural Mechanization, Ministry of Agriculture and Rural Affairs, Nanjing 210014, China; College of Mechanics and Materials, Hohai University, Nanjing 211100, China; College of Engineering, Nanjing Agricultural University, Nanjing 210031, China
2 College of Mechanics and Materials, Hohai University, Nanjing 211100, China
3 Nanjing Institute of Agricultural Mechanization, Ministry of Agriculture and Rural Affairs, Nanjing 210014, China
4 College of Mechanics and Materials, Hohai University, Nanjing 211100, China; Jiangsu Key Laboratory for Light Metal Alloys, Nanjing Yunhai Special Metals Co., Ltd., Nanjing 211200, China