1. Introduction
The development of more sustainable solutions to environmental concerns is a common goal that encompasses materials science technologies. Among them, paint and coating systems focus on the use of less toxic components while preserving high physical/chemical and mechanical properties [1,2,3]. This need is particularly felt in shipbuilding, since the steel used for hull construction is subject to corrosion in seawater and biofouling while also having to meet the requirement to operate at extremely low temperatures [4].
A suitable strategy to enhance the functional features of organic coatings entails the addition of nanomaterials such as SiO2, TiO2, ZnO, Al2O3, CaCO3, and CeO2. The incorporation of targeted nanopowders into a polymeric matrix may influence the coating performance and optimize the mechanical, chemical, and optical properties [5]. Some studies reported the functional performance of nanoparticles of SiO2, Zn, and Fe2O3 as anti-corrosive agents as well as the mechanical properties of modifiers for epoxy [6] and silane-based sol–gel [7] coatings. The peculiar properties of nanoparticles have been utilized in the coating industry to improve the physical, mechanical, and chemical properties of organic coatings [8,9,10,11].
A great emphasis is placed on the utilization of easily available starting materials such as commercial silica gel, whose high specific surface area combined with its high thermal and chemical stability allows a wide range of surface modifications. Another example of a commercial nanopowder for the preparation of functional paints and coatings is titanium dioxide, which emerged in the field of photocatalysis for environmental applications [12]. The demand for effective solutions to address marine biofouling challenges has driven the advancement of antifouling and anticorrosion coatings, often incorporating nanocomposite materials with biocidal agents or utilizing the fouling release mechanism [13,14,15,16,17,18]. More broadly, the development of nanocomposite materials with antimicrobial and antifouling characteristics is a widely studied area, with applications across diverse research domains, including the creation of biomedical devices, water purification systems, food packaging, and marine equipment. The biocide action of some metal and metal oxide nanoparticles (NPs), in particular silver (Ag) NPs, copper (CuO), and zinc oxide (ZnO), is well known [19,20]. The studies on these materials are still increasing due to their broad-spectrum antimicrobial properties.
In general, they can act by adhesion onto the bacterial surface followed by the destabilization of the cell wall, inducing modifications of membrane permeability or causing toxicity and oxidative stress by the generation of reactive oxygen species (ROS). Recently, EuChems (
The final materials (SiO2-NH2-Fe and TiO2-NH2-Fe) were then characterized and employed for the preparation of paint formulations which were applied to the surface of metal prototypes.
The surface properties of the resulting coatings, deposited on DH 36 steel plates, were evaluated through the determination of thickness, water wettability, roughness, and cross-cut adhesion tests. The antimicrobial activity of the iron amino-functionalized materials was also tested, as proof of concept, to monitor the growth of some bacterial strains.
2. Materials and Methods
2.1. Materials and Paint Formulation Synthetic Procedures
Plates of DH36 high-strength structural steel, conforming to the ASTM A131/A131M-19 standard [34] or to the equivalent grade ABS DH36, were selected as the substrate for depositing and testing the coatings.
The chemical composition limits, according to ASTM A131/A131M-19 Designation are shown in Table 1.
Silica and titania were functionalized with aminopropyl groups adopting a grafting method. In a typical procedure, a mixture of 1.00 g of calcined silica or titania in 15.0 mL of absolute ethanol and 1.00 mL of 3-aminopropyl triethoxysilane (APTES) was refluxed overnight. The materials were filtered in vacuo, washed with ethanol, and dried overnight at 120 °C. Iron (5% w/w) was supported by a wet impregnation procedure. In a typical procedure, iron nitrate nonahydrate (Fe(NO3)3·9H2O, 543 mg) was dissolved in 10 mL of water and added to aminopropyl silica or titania (1.5 g). The mixture was stirred overnight at room temperature, then it was filtered and washed with water.
Plates of DH36 high-strength structural steel, conforming to ASTM standards or the equivalent grade ABS DH36, were selected as the substrate for depositing and testing the coatings.
The preparation of paint formulation was carried out by mixing the Fe-based powder with a commercially available two-component polyamine-cured pure epoxy coating (Safeguard Universal ES, Jotun, “tie-coat, Jotun Italia Srl, Muggia, Trieste, Italy). Component A (6 g, Safeguard Universal ES Comp. A), component B (1.2 g, Safeguard Universal ES Comp. B), the diluent (0.36 g, Thinner n° 17), and SiO2-NH2-Fe or TiO2-NH2-Fe solid (75.6 mg) were mechanically mixed into a PP vessel by using a flat brush until a homogeneous paint was obtained. The as-obtained SiO2- or TiO2-based formulations were deposited on the surface of a metal plate (structural steel DH36 150 × 75 mm, thickness 5 mm) with a flat brush. The day before the application of the Fe-based formulation, a pristine metal specimen bearing a primer coating was treated with a tie coat paint as the basic surface (Jotun, Sandefjord, Norway) and dried overnight at room temperature.
Table 2 lists the four types of materials used in this study, with the code, description, and details.
Figure 1a–d show the four coatings of this study after the deposition on the structural steel DH36 plate (geometry of 150 × 75 mm, thickness 5 mm); each picture geometry is specified in Figure 1e (red colour bars). Each coated structural steel plate was marked with a pencil that marked the various points to create an internal grid (14 cm × 6 cm; see the black colour bars in Figure 1e). Thickness measurements were taken on these grid points to create a mapping extended to the entire sample (see Figure 1e where the intersection point of the vertical white lines with the horizontal white lines, highlighted on the red substrate, defines the exact point where the thickness value is measured that will be reported in the thickness maps discussed in Section 3).
2.2. Chemical Characterization
The textural properties of the materials were examined with a Micromeritics ASAP2020 Plus 1.03 (Micromeritics, Ottawa, ON, Canada). The specific surface areas of the samples were evaluated through the analysis of the N2 adsorption isotherm at 77 K by using the BET method in the standard pressure range of 0.05–0.3 p/p0. The total pore volume, Vp, was calculated from the amount of nitrogen adsorbed at a relative pressure of 0.998, whereas mesopore size distribution values and mesopore volumes were estimated by applying the BJH model in the range of p/p0 of 0.1–0.98.
The thermogravimetric analysis of the samples was carried out in air using the TGA 1 Star System of Mettler Toledo (Mettler Toledo, Schwerzenbach, Switzerland). About 10 mg of sample was heated from room temperature to 100 °C, left at this temperature for 30 min, and then heated to 1000 °C at a rate of 10 °C/min in 40 mL/min of air.
The X-ray photoelectron spectroscopy (XPS) analyses were performed with a VG Microtech ESCA 3000 Multilab (VG Microtech/VG Scientific, East Grinstead, West Sussex, UK), equipped with a dual Mg/Al anode. Unmonochromatic Al Ka radiation (1486.6 eV) was used as the excitation source. The sample powders were mounted on a double-sided adhesive tape. The pressure in the analysis chamber was in the range of 10–8 Torr during data collection. The constant charging of the samples was removed by referencing all the energies to the C 1 s binding energy set at 285.1 eV. Analyses of the peaks were performed with the CasaXPS 2.3.26 software.
2.3. Physical/Mechanical Characterization
The four coatings were physically and mechanically characterized by thickness evaluation, wettability tests, and cross-section tests (adhesion strength evaluation before, at t = 0 days, and after, at t = 30 days, a period of immersion in seawater).
To measure the thickness of metal specimens deposited with coatings, a digital thickness gauge SA-MA Tools SA8850 (SAMA Italia, Viareggio, Italy) was utilized. A grid (14 cm × 6 cm; see the black color values in Figure 1e) was created on the metal specimen to acquire, at the intersection points, the different thickness values for the whole specimen. Thickness measurements were taken at each grid point by positioning the probe perpendicular to the specimen. To give a chromatic idea of the distribution of thickness values of the analyzed samples, chromatographic maps were created using a 14 × 6 matrix with the graphic processing software Origin © 2.019. The average of all the measurements was subsequently calculated.
The measurements of surface roughness were carried out using the portable and compact Surftest SJ-210 Series 178 roughness tester (Mitutoyo S.r.l., Milan, Italy), according to Equation:
where Ra denotes the arithmetic mean of the absolute values of the deviations of the evaluation profile (Yi) from the mean line. The data presented are the average values from nine measurements for each type of sample.The Wenzel contact angle (θw) and that of Young (θy, not dependent on the roughness) were assessed using the θ/2 method (prototype instrument—Engineering Department, Messina University) by measuring the contact angle of a 1 μL drop of deionized water placed on the horizontal surface of the sample, in accordance with ASTM D7334 [35] and Equation:
where (d) is the diameter (in mm) and (h) is the height (in mm) of the drop. The data presented are the average values obtained from ten measurements for each sample [36].The adhesion resistance of antifouling coatings was evaluated in seawater in accordance with ASTM D870-97 standards [37]. The samples were placed in aquarium tanks (rectangular shape of 30 × 20 cm, height of 20.3 cm) and completely submerged in seawater. To replicate the movement of seawater, a submerged aquarium pump (flow rate Q = 200 L/h, pipe diameter = 8 mm, flow velocity exiting the pipe = 1.11 m/s, flow velocity along the cross section = 0.0009 m/s) with a filter was utilized to ensure constant water recirculation over the surfaces. The water temperature was maintained at 24 °C, while the ambient temperature was kept at 23 °C. The seawater was refreshed every two weeks (Figure 2).
The samples were subsequently examined for potential bubble formation, softening, and loss of adhesion using the cross-cut test (Cross Hatch Adhesion Tester by Sama Tools—SADT502-5, SAMA Italia, Viareggio, Italy) before and after immersion in seawater after 1 month.
This method employs a suitable cutting tool with a blade space of 2 mm (for coatings of 60–120 microns) to score the coating down to the substrate. Specifically, on a 15 × 7.5 cm substrate, two cuts are made that intersect at 90 degrees, creating square-shaped grid patterns with four intersections on the substrate of 1.8 × 1.8 cm (see Figure 3a). The cross-cut area is then examined for any adhesion issues. The relevant standards for this test are D 3359-09e2 [38] and ISO 2409:2007 [39] (see Figure 3b–g).
2.4. Microtox Assay
Microtox® toxicity tests were carried out on SiO2-NH2-Fe and TiO2-NH2-Fe materials. The Microtox® toxicity tests were conducted using the luminescent bacterium Vibrio fisheri according to the standard procedures of the EN12457 protocol with the following modifications. The values of bioluminescence inhibition (indirect index of toxicity values) were reported as the effective concentrations (100 mg L−1) of toxicants resulting in a 50% decrease in bioluminescence (EC50). The EC50 with 95% confidence intervals was calculated, after 15 and 30 min of exposition, following the procedures outlined in the Microtox® System Operating Manual (Microtox, Columbus, OH, USA, 2003). Each biocidal sample was compared with a reference un-toxicity matrix.
2.5. Bacteria, Culture Conditions, and Microbiological Tests
Microbial strains: three bacterial strains, namely, Pseudoalteromonas sp., Alteromonas sp., and Pseudomonas sp., were used in this study. All three were isolated from the marine environment and maintained in the culture collection of the Institute of Biological Resources and Marine Biotechnology (IRBIM)-CNR of Messina (Messina, Italy).
Microbial preparation: starter cultures were carried out by inoculating microbial cells into 10 mL of Marine Broth (MB; Difco, Milan) mineral medium. Cultures were grown in a rotary shaker (New Brunswick C24KC, Edison, NJ, USA; 150 rpm) at 20 ± 1 °C for 5 days. Mid-exponential-phase grown cells were harvested by centrifugation at 10.000× g for 10 min, washed twice with sterile MB, and inoculated into different 100 mL sterile Erlenmeyer flasks each containing 50 mL of Marine Broth.
Evaluation of the biocidal activity of the new functionalized coatings: mid-exponential-phase grown cells were harvested a second time as previously described and inoculated at a final concentration of 0.1 of optical density (OD600 nm) in a sterile medium supplemented with 100 mg L−1 of SiO2-NH2-Fe and TiO2-NH2-Fe materials. The cultures were incubated at 20 ± 1 °C for 9 days, with shaking (150× g, New Brunswick C24KC, Edison, NJ, USA). All experiments were carried out in triplicate. At the beginning of experimentation and regular intervals (3 days), the growth (biomass variations) of the cultures in this study was routinely assessed indirectly by measuring the turbidity (OD600 nm) using a UV–visible spectrophotometer (Shimadzu UV-160, Markham, ON, Canada).
3. Results and Discussion
The synthesis of Fe-based powders, as reported in Scheme 1, was carried out through the covalent grafting of (3-aminopropyl)triethoxysilane (APTES) onto the surface of commercial SiO2 or TiO2 in ethanol. The obtained hybrid materials SiO2-NH2 and TiO2-NH2 were used as supports for the immobilization of iron sites, which was performed by a wet impregnation procedure using Fe(NO3)3·9H2O as metal precursor. The final solids were labeled as SiO2-NH2-Fe and TiO2-NH2-Fe.
The thermogravimetric analysis (TGA) of SiO2-NH2-Fe and TiO2-NH2-Fe showed, in both cases, good thermal stability at 180 °C (Figure 4).
The higher organic loading of SiO2-NH2-Fe can be ascribed to the specific surface area of pristine SiO2 (SSABET 545 m2/g) when compared to bare TiO2 (SSABET 56 m2/g). The specific surface area value of silica implies a good -OH availability that is pivotal for the condensation of APTES functional groups. N2 physisorption measurements (Figure 5) were carried out on SiO2-NH2 (SSABET 208 m2/g), SiO2-NH2-Fe (SSABET 190 m2/g), TiO2-NH2 (SSABET 59 m2/g), and TiO2-NH2-Fe (SSABET 48 m2/g).
The XPS analysis was performed to analyze the surface of the synthesized additives. The survey spectra (see Figure 6A) show for both materials the peaks due to the bare supports. In addition, for SiO2-NH2-Fe, it is possible to appreciate the N1s peak due to the presence of the propylNH2 functionalization. The presence of Fe is not evidenced in the survey spectra. In order to better analyze the materials, the single regions (Fe2p and N1s) were recorded and the results are shown in Figure 6B,C, respectively. The presence of iron is confirmed by the presence of the characteristic Fe2p doublet in both materials. The low intensity of the peaks and the natural complexity of the Fe2p emission [40] make it difficult to evaluate the oxidation state of iron; however, the position and the shape of the profile are consistent with the iron in the +3 oxidation state. The analysis of the N1s region, showing the presence of a peak at 399.8 eV typical of the amino group [33], confirms that the surface of SiO2-NH2-Fe has been functionalized. By contrast, the absence of a visible N1s-related peak in the TiO2-NH2-Fe scan indicates that, in this sample, the functionalization was less effective.
Regarding the ecotoxicological assays, the Microtox tests show that SiO2-NH2-Fe and TiO2-NH2-Fe samples do not cause significant bioluminescence decay in Vibrio fischeri (Table 3). In the EN12457 protocol, the Microtox® bioluminescent assay assessed in water typically shows an underestimated sensitivity to highly hydrophobic chemicals. This is primarily because these compounds have extremely low solubility in water and almost irreversible adsorption of matrix-like sediments.
The growth curves of the bacterial strains were monitored by measuring the optical density (OD) at 600 nm in the presence of two matrices: SiO2-NH2-Fe and TiO2-NH2-Fe. Measurements were taken over 9 days, with assessments every 3 days (Figure 7).
Strains grown with SiO2-NH2-Fe showed similar growth patterns initially, with the Alteromonas sp. strain peaking at day 6 before stabilizing. Pseudoalteromonas sp. also followed this trend, peaking at day 9, while Pseudomonas sp. exhibited the highest growth at the end. In contrast, the TiO2-NH2-Fe environment yielded higher growth for both Pseudoalteromonas and Pseudomonas strains. Pseudoalteromonas sp. reached values of 0.5 to 0.6 on days 3 and 6, then increased to about 0.9 by day 9. Pseudomonas sp. showed fluctuating growth initially but also increased to approximately 0.9 on day 9. The Alteromonas strain grew from 0.1 on day 0 to 0.6 on day 9.
In summary, bacterial strains demonstrated better growth in the TiO2-NH2-Fe suspension compared to SiO2-NH2-Fe.
These preliminary tests assessed the antimicrobial activity of the iron amino-functionalized materials and highlighted their promising properties.
The antibacterial mechanism of Fe(III) against bacteria was studied by Sun et al., who reported that bacteria could adsorb Fe(III) and reduce it to Fe(II) [22].
As noted by Videira-Quintela et al. [41], the antibacterial effect can be related to Fe(II) ions, which produce reactive oxygen species (ROS) including hydroxyl radicals (OH·), leading to bacterial damage and growth inhibition [42,43]. Additionally, hydroxyl radical production likely occurs via the Fenton reaction: Fe(II) + H2O2 → Fe(III) + OH + OH−, where Fe(II) reacts with hydrogen peroxide (H2O2), generated through the dismutation of superoxide (2O2− + 2H+ → H2O2 + O2) during Fe(II) autoxidation [44].
The antibacterial effect of TiO2 nanoparticles modified with APTES is documented by Rokicka-Konieczna [30], whereas we developed corresponding functional materials based on SiO2 and TiO2 with enhanced functional iron-based sites.
The antibacterial action of SiO2 nanoparticles operates through various mechanisms, such as adsorption and membrane disruption, the generation of ROS, and intracellular penetration. These processes work in concert to enhance the bactericidal effect of SiO2 nanoparticles as proof of their promise of antimicrobial activity [45].
The enhanced antibacterial activity of SiO2-NH2-Fe compared to TiO2-NH2-Fe could be attributed to both the higher loading of amino groups in SiO2-NH2-Fe and the greater specific surface area of silica, which facilitates better adsorption onto bacterial cell surfaces. The adsorption process involves electrostatic interactions between the hydroxyl groups and the bacterial membrane, as well as between the amino groups [31] and the bacterial membrane. Upon adsorption, the designed nanomaterials interact with the lipid bilayer of the bacterial membrane, disrupting its integrity and structure. This damage increases membrane permeability, causing leakage of essential cellular components like ions and cytoplasmic molecules. The loss of these vital elements disrupts the bacterial cells’ homeostasis and function, ultimately resulting in cell death [45].
Functional additives were mechanically dispersed in a commercial tie coat to be applied on the surface of metal prototype plates by using a flat brush, according to the description in Section 2.
The average thickness values are listed in Table 4. The value of the commercial tie coat and topcoat was 498 microns and 515 microns, respectively. As expected, the thickness value improved after the addition of the two topcoats (653 microns (Si-Top) and 674 microns (Ti-Top)).
Figure 8 shows the thickness distribution map calculated on the 6 cm × 14 cm surface of the metal plate.
Generally, all the maps reveal a thickness distribution that is not always homogeneous. There is a greater inhomogeneity in the Si-Top compared to the other topcoats. This is due to the manual deposition of the coatings.
Table 4 summarizes the roughness Ra values of the coatings. Figure 9 shows that the C-Top coating is much rougher (Ra = 5.78 μm) than the other substrates.
From the graph below and the values detailed in Table 4, it can be seen how the contact angle θw (°) and θy (°/μm) of the coatings, except for C-Top, which is hydrophilic (θw = 73°, θy = 87°), have hydrophobic characteristics, that is, they have a contact angle greater than 90°.
In particular, Ti-Top exhibits the highest contact angle value, resulting in the more hydrophobic coatings among the four investigated (Figure 10).
The cross-cut test (refer to Figure 11) showed that three coatings—C-Tie, C-Top, and Si-Top—exhibited the highest adhesion rating of 5B/0, according to the evaluation scale presented in Figure 3, before undergoing the seawater resistance test. In contrast, the Ti-Top coating had a lower adhesion rating of 4B/1.
The high adhesion value (5B/0) of the C-Tie, C-Top, and Si-Top coating agrees with the finding of other authors who studied similar epoxy-based coatings containing ZnO-APTES, and they proved that the adhesin power was the highest [46,47].
After 30 days of testing in seawater, the adhesive capacity of all coatings decreases. The commercial topcoat demonstrates the lowest resistance among all the coatings analyzed because it drops from a value of 5B/0 to a value of 2B/3 (see Figure 3).
The most resistant coating, Si-Top, decreases from a value of 5B/0 to 4B/1. In comparison, the Ti-Top coating, which is less resistant, drops further from a value of 4B/1 to 3B/2. Therefore, the Si-Top antifouling coating is the best option regarding adhesive capacity and is also less hydrophobic than the Ti-Top coating.
The enhanced performance of Si-Top, along with its increased hydrophilicity, can be attributed to the higher concentration of amino groups in the SiO2-based nanopowder with respect to the titania-supported one. The increased loading of functional groups is associated with the large surface area of the SiO2 support, which, in turn, results in a higher density of -OH groups, further enhancing the hydrophilic properties.
Furthermore, manual deposition involves human error due to the operator, his/her manual skills, and his/her experience in carrying out manual deposition work. In our work, the coatings were always deposited by the same operator and under the same temperature and pressure conditions. That is, the operator carried out the deposition in an extremely short time to contain any variables, and using the same type of brush (flat).
Although we did not obtain a deposition that was entirely homogeneous, as can be seen from the images in Figure 8 (due to understandable human error), our coatings still managed to adhere well to the metal substrate, as demonstrated by the results of the mechanical tests (Table 4). Therefore, the yield would certainly be increased if a deposition were to be carried out with more precise technologies (for example, spray coating), further improving the already good performance of our coatings.
4. Conclusions
This article focused on novel coatings developed to protect DH 36 steel plates widely used in offshore structures and shipbuilding. SiO2 and TiO2 were modified with amino groups to create hybrid materials for immobilizing iron sites. These were incorporated into paint formulations, which were applied to steel prototype plates. The coatings’ properties, including thickness, water wettability, roughness, and adhesion, were tested, along with their performance in seawater degradation, and microbiological tests.
The main findings were as follows:
SiO2-NH2-Fe powders exhibited better antibacterial performance compared to TiO2-NH2-Fe powders, making SiO2-NH2-Fe a more suitable candidate for antifouling applications;
The higher adhesion and lower surface roughness exhibited by the SiO2-based material compared to the TiO2-based material, together with its hydrophobicity (θ > 90°), further support its potential to improve the durability and performance of coatings in marine environments;
The application of a primer coating followed by a tie coat containing TiO2-NH2-Fe or SiO2-NH2-Fe powders on DH 36 steel plates eliminates the need for an additional topcoat, presenting a notable strategic advantage for simplifying the coating process while maintaining effective steel surface protection.
Conceptualization, M.L.T., C.C., V.L.P., C.S., A.V., S.C. and L.F.L.; methodology, M.L.T., C.C., V.L.P., C.S., A.V., S.C. and L.F.L.; validation, M.L.T., C.C., V.L.P., C.S., A.V., S.C. and L.F.L.; formal analysis, M.L.T., C.C., V.L.P., C.S., A.V., S.C. and L.F.L.; investigation, M.L.T., C.C., V.L.P., C.S., A.V., S.C. and L.F.L.; resources, A.V. and L.F.L.; data curation, M.L.T., C.C., V.L.P., C.S., A.V., S.C. and L.F.L.; writing—original draft preparation, M.L.T., C.C., V.L.P., C.S., A.V., S.C. and L.F.L.; writing—review and editing, M.L.T., C.C., V.L.P., C.S., A.V., S.C. and L.F.L.; visualization, A.V. and L.F.L.; supervision, A.V. and L.F.L.; funding acquisition, A.V. and L.F.L. All authors have read and agreed to the published version of the manuscript.
The data presented in this study are available on request from the corresponding authors.
F. Giordano (ISMN-CNR, Italy) and N. Gallì (ISMN-CNR, Italy) are acknowledged for technical support in the laboratory and for carrying out XRD and BET analyses, respectively. G. Napoli (ISMN-CNR) is acknowledged for the financial management of funding. The authors thank NAVTEC (Consorzio di Ricerca per l’Innovazione Tecnologica, Sicilia, Trasporti navali, commerciali e da diporto s.c.a.r.l) for research funding, grant number ARS01_00293 PON2014-2020 of research project “Thalassa” (TecHnology And materials for safe low consumption and low lifecycle cost veSSels And crafts).
The authors declare no conflicts of interest.
Footnotes
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.
Figure 1. Materials of this study: C-Top (a), C-Tie (b), Si-Top (c), and Ti-Top (d) after their deposition on the structural steel DH36 with the internal measuring grid for the detection of thickness maps (6 cm × 14 cm): red colour bars refer to external geometry and black colour bars refers to the internal grid (e).
Figure 2. Different views of the set-up for the measurement of the resistance to seawater of the coatings deposited on structural steel plate samples and fully immersed in seawater: low side (a), top (b), high side (c).
Figure 3. Geometry of a square-shaped grid generated during the cross-cut test (a) and ASTM/ISO standards: 5B/0 (b), 4B/1 (c), 3B/2 (d), 2B/3 (e), 1B/4 (f), 0B/5 (g) detachment types.
Figure 5. N2 adsorption/desorption isotherms of SiO2-NH2-Fe, SiO2-NH2-Fe, TiO2-NH2, and TiO2-NH2-Fe.
Figure 6. XPS spectra of SiO2-NH2-Fe and TiO2-NH2-Fe: (A) survey spectra; (B) Fe2p region; and (C) N1s region.
Figure 7. Growth of bacterial strains, measured as optical density (OD600 nm), in the presence of SiO2-NH2-Fe and TiO2-NH2-Fe. Error bar (5%).
Figure 8. Thickness maps of C-Tie-498 μm (a), C-Top 515 μm (b), Si-Top 653 μm (c), and Ti-Top 674 μm (d).
Figure 9. Typical roughness profiles of the substrates of the coatings deposited on metal.
Figure 11. Cross-cut test results of the coatings: (a) C-Tie; (b) C-Top; (c) Si-Top; (d) Ti-Top; and after 1 month of immersion in seawater: (e) C-Tie; (f) C-Top; (g) Si-Top; (h) Ti-Top.
Composition limits for ASTM DH36 high-strength structural steel (weight %).
C | Mn | Si | P | S | Al | Cb (Nb) | Ti | Cu | Cr | Ni | Mo | Ca | Fe |
---|---|---|---|---|---|---|---|---|---|---|---|---|---|
0.18 | 0.9–0.16 | 0.1–0.5 | 0.035 | 0.035 | 0.015 | 0.02–0.05 | 0.02 | 0.35 | 0.20 | 0.40 | 0.08 | 0.05 | Bal. |
Codes and materials of this study.
Code | Typology of Material | Description | Details |
---|---|---|---|
C-Top | Sea Quantum Ultra S | Commercial topcoat | Cutting-edge, single-component antifouling with silyl acrylate chemical reaction |
C-Tie | Safeguard Universal ES, Jotun “tie-coat” | Commercial tie coat | Two-component epoxy-vinyl with polyamide hardener (5:1) |
Si-Top | Si-Tie + SiO2-NH2-Fe | Commercial Tiecoat + our SiO2-based additive | |
Ti-Top | Ti-Tie + TiO2-NH2-Fe | Commercial Tiecoat + our TiO2-based additive |
Measurement of Microtox® toxicity on SiO2-NH2-Fe and TiO2-NH2-Fe materials.
Sample | Concentration (mg L−1) | Matrix | EC50 | EC50 |
---|---|---|---|---|
SiO2-NH2-Fe | 100 | Powder | >100 | >100 |
TiO2-NH2-Fe | 100 | Powder | >100 | >100 |
Thickness, roughness, wettability, and adhesion power of all coatings.
Sample | Thickness | Wenzel/Roughness/Young | Cross-Cut Test | |||
---|---|---|---|---|---|---|
θw [°] | Ra [μm] | θy [°/μm] | (t = 0 days) | (t = 30 days) | ||
C-Tie | 498 ± 96 | 93.47 ± 1.62 | 1.20 ± 0.08 | 92.89 ± 1.62 | 5B/0 | 4B/1 |
C-Top | 515 ± 52 | 73.04 ± 0.73 | 5.78 ± 0.06 | 87.11 ± 0.73 | 5B/0 | 2B/3 |
Si-Top | 653 ± 73 | 91.65 ± 1.58 | 1.21 ± 0.07 | 91.36 ± 1.58 | 5B/0 | 4B/1 |
Ti-Top | 674 ± 64 | 96.37 ± 1.75 | 1.30 ± 0.05 | 94.90 ± 1.75 | 4B/1 | 3B/2 |
References
1. Akhter, P.; Arshad, A.; Hussain, M. A review on environmental impacts of paints and strategies for producing eco-friendly-paints. Int. J. Environ. Sci. Technol.; 2025; 22, 555. [DOI: https://dx.doi.org/10.1007/s13762-024-05760-z]
2. Fanicchia, F.; Karlsdottir, S.N. Research and Development on Coatings and Paints for Geothermal Environments: A Review. Adv. Mater. Technol.; 2023; 8, 2202031. [DOI: https://dx.doi.org/10.1002/admt.202202031]
3. Faccini, M.; Bautista, L.; Soldi, L.; Escobar, A.M.; Altavilla, M.; Calvet, M.; Domènech, A.; Domínguez, E. Environmentally Friendly Anticorrosive Polymeric Coatings. Appl. Sci.; 2021; 11, 3446. [DOI: https://dx.doi.org/10.3390/app11083446]
4. Zhao, W.; Feng, G.; Zhang, M.; Ren, H.; Sinsabvarodom, C. Effect of low temperature on fatigue crack propagation rates of DH36 steel and its butt weld. Ocean. Eng.; 2020; 196, 106803. [DOI: https://dx.doi.org/10.1016/j.oceaneng.2019.106803]
5. Dashtizadeh, A.; Abdouss, M.; Mahdavi, H.; Khorassani, M. Acrylic coatings exhibiting improved hardness, solvent resistance and glossiness by using silica nano-composites. Appl. Surf. Sci.; 2011; 257, pp. 2118-2125. [DOI: https://dx.doi.org/10.1016/j.apsusc.2010.09.060]
6. Shi, X.; Nguyen, T.A.; Suo, Z.; Liu, Y.; Avci, R. Effect of nanoparticles on the anticorrosion and mechanical properties of epoxy coating. Surf. Coat. Technol.; 2009; 204, pp. 237-245. [DOI: https://dx.doi.org/10.1016/j.surfcoat.2009.06.048]
7. Phanasgaonkar, A.; Raja, V.S. Influence of curing temperature, silica nanoparticles- and cerium on surface morphology and corrosion behaviour of hybrid silane coatings on mild steel. Surf. Coat. Technol.; 2009; 203, pp. 2260-2271. [DOI: https://dx.doi.org/10.1016/j.surfcoat.2009.02.020]
8. Jalili, M.M.; Moradian, S.; Dastmalchian, H.; Karbasi, A. Investigating the variations in properties of 2-pack polyurethane clear coat through separate incorporation of hydrophilic and hydrophobic nano-silica. Prog. Org. Coat.; 2007; 59, pp. 81-87. [DOI: https://dx.doi.org/10.1016/j.porgcoat.2007.01.018]
9. Amerio, E.; Fabbri, P.; Malucelli, G.; Messori, M.; Sangermano, M.; Taurino, R. Scratch resistance of nano-silica reinforced acrylic coatings. Prog. Org. Coat.; 2008; 62, pp. 129-133. [DOI: https://dx.doi.org/10.1016/j.porgcoat.2007.10.003]
10. Sangermano, M.; Malucelli, G.; Amerio, E.; Priola, A.; Billi, E.; Rizza, G. Photopolymerization of epoxy coatings containing silica nanoparticles. Prog. Org. Coat.; 2005; 54, pp. 134-138. [DOI: https://dx.doi.org/10.1016/j.porgcoat.2005.05.004]
11. Barna, E.; Bommer, B.; Kürsteiner, J.; Vital, A.; Trzebiatowski, O.v.; Koch, W.; Schmid, B.; Graule, T. Innovative, scratch proof nanocomposites for clear coatings. Compos. Part A Appl. Sci. Manuf.; 2005; 36, pp. 473-480. [DOI: https://dx.doi.org/10.1016/j.compositesa.2004.10.014]
12. Chen, M.C.; Koh, P.W.; Ponnusamy, V.K.; Lee, S.L. Titanium dioxide and other nanomaterials based antimicrobial additives in functional paints and coatings: Review. Prog. Org. Coat.; 2022; 163, 106660. [DOI: https://dx.doi.org/10.1016/j.porgcoat.2021.106660]
13. Scolaro, C.; Liotta, L.F.; Calabrese, C.; Marcì, G.; Visco, A. Adhesive and Rheological Features of Ecofriendly Coatings with Antifouling Properties. Polymers; 2023; 15, 2456. [DOI: https://dx.doi.org/10.3390/polym15112456] [PubMed: https://www.ncbi.nlm.nih.gov/pubmed/37299255]
14. Scurria, A.; Scolaro, C.; Sfameni, S.; Di Carlo, G.; Pagliaro, M.; Visco, A.; Ciriminna, R. Towards AquaSun practical utilization: Strong adhesion and lack of ecotoxicity of solar-driven antifouling sol-gel coating. Prog. Org. Coat.; 2022; 165, 106771. [DOI: https://dx.doi.org/10.1016/j.porgcoat.2022.106771]
15. Seraj, S.; Mohammadi, T.; Tofighy, M.A. 15-Polymer nanocomposite films and coatings for antifouling applications. Polymer Nanocomposite Films and Coatings; Pandey, M.; Deshmukh, K.; Hussain, C.M. Woodhead Publishing: Cambridge, UK, 2024; pp. 525-558.
16. Padmavathi, A.R.; Murthy, P.S.; Das, A.; Veeramani, P.; Rao, T.S. Inorganic nanoparticle embedded Polydimethyl siloxane nanocomposites for biofouling mitigation. Surf. Interfaces; 2021; 25, 101171. [DOI: https://dx.doi.org/10.1016/j.surfin.2021.101171]
17. Hu, P.; Xie, Q.; Ma, C.; Zhang, G. Silicone-Based Fouling-Release Coatings for Marine Antifouling. Langmuir; 2020; 36, pp. 2170-2183. [DOI: https://dx.doi.org/10.1021/acs.langmuir.9b03926]
18. Liang, H.; Shi, X.; Li, Y. Technologies in Marine Antifouling and Anti-Corrosion Coatings: A Comprehensive Review. Coatings; 2024; 14, 1487. [DOI: https://dx.doi.org/10.3390/coatings14121487]
19. Calabrese, C.; La Parola, V.; Testa, M.L.; Liotta, L.F. Antifouling and antimicrobial activity of Ag, Cu and Fe nanoparticles supported on silica and titania. Inorganica Chim. Acta; 2022; 529, 120636. [DOI: https://dx.doi.org/10.1016/j.ica.2021.120636]
20. Izzi, M.; Sportelli, M.C.; Torsi, L.; Picca, R.A.; Cioffi, N. Synthesis and Antimicrobial Applications of ZnO Nanostructures: A Review. ACS Appl. Nano Mater.; 2023; 6, pp. 10881-10902. [DOI: https://dx.doi.org/10.1021/acsanm.3c01432]
21. Chekini, M.; Krivoshapkina, E.; Shkodenko, L.; Koshel, E.; Shestovskaya, M.; Dukhinova, M.; Kheiri, S.; Khuu, N.; Kumacheva, E. Nanocolloidal Hydrogel with Sensing and Antibacterial Activities Governed by Iron Ion Sequestration. Chem. Mater.; 2020; 32, pp. 10066-10075. [DOI: https://dx.doi.org/10.1021/acs.chemmater.0c03362]
22. Sun, H.-Q.; Lu, X.-M.; Gao, P.-J. The exploration of the antibacterial mechanism of Fe3+ against bacteria. Braz. J. Microbiol.; 2011; 42, pp. 410-414. [DOI: https://dx.doi.org/10.1590/S1517-83822011000100050]
23. Pansuriya, P.B.; Patel, M.N. Iron(III) complexes: Preparation, characterization, antibacterial activity and DNA-binding. J. Enzym. Inhib. Med. Chem.; 2008; 23, pp. 230-239. [DOI: https://dx.doi.org/10.1080/14756360701474657]
24. Ben Abdelhadi, A.; Rodríguez-Sánchez, S.; Ouarsal, R.; Saadi, M.; El Ammari, L.; Morley, N.; El Bali, B.; Gómez-Torres, Ó.; Lachkar, M.; Douhal, A. Synthesis, characterization, and magnetic and antibacterial properties of a novel iron(iii) complex (CH3)2NH2[Fe(phen)Cl4]. Mater. Adv.; 2024; 5, pp. 3058-3066. [DOI: https://dx.doi.org/10.1039/D3MA00971H]
25. Kwaśniewska, D.; Chen, Y.-L.; Wieczorek, D. Biological Activity of Quaternary Ammonium Salts and Their Derivatives. Pathogens; 2020; 9, 459. [DOI: https://dx.doi.org/10.3390/pathogens9060459] [PubMed: https://www.ncbi.nlm.nih.gov/pubmed/32531904]
26. Marzullo, P.; Gruttadauria, M.; D’Anna, F. Quaternary Ammonium Salts-Based Materials: A Review on Environmental Toxicity, Anti-Fouling Mechanisms and Applications in Marine and Water Treatment Industries. Biomolecules; 2024; 14, 957. [DOI: https://dx.doi.org/10.3390/biom14080957] [PubMed: https://www.ncbi.nlm.nih.gov/pubmed/39199346]
27. Nemeş, N.S.; Ardean, C.; Davidescu, C.M.; Negrea, A.; Ciopec, M.; Duţeanu, N.; Negrea, P.; Paul, C.; Duda-Seiman, D.; Muntean, D. Antimicrobial Activity of Cellulose Based Materials. Polymers; 2022; 14, 735. [DOI: https://dx.doi.org/10.3390/polym14040735] [PubMed: https://www.ncbi.nlm.nih.gov/pubmed/35215647]
28. Shao, W.; Wu, J.; Liu, H.; Ye, S.; Jiang, L.; Liu, X. Novel bioactive surface functionalization of bacterial cellulose membrane. Carbohydr. Polym.; 2017; 178, pp. 270-276. [DOI: https://dx.doi.org/10.1016/j.carbpol.2017.09.045]
29. Koshani, R.; Eiyegbenin, J.E.; Wang, Y.; van de Ven, T.G.M. Synthesis and characterization of hairy aminated nanocrystalline cellulose. J. Colloid Interface Sci.; 2022; 607, pp. 134-144. [DOI: https://dx.doi.org/10.1016/j.jcis.2021.08.172]
30. Rokicka-Konieczna, P.; Wanag, A.; Sienkiewicz, A.; Kusiak-Nejman, E.; Morawski, A.W. Antibacterial effect of TiO2 nanoparticles modified with APTES. Catal. Commun.; 2020; 134, 105862. [DOI: https://dx.doi.org/10.1016/j.catcom.2019.105862]
31. Bouazizi, N.; Vieillard, J.; Samir, B.; Le Derf, F. Advances in Amine-Surface Functionalization of Inorganic Adsorbents for Water Treatment and Antimicrobial Activities: A Review. Polymers; 2022; 14, 378. [DOI: https://dx.doi.org/10.3390/polym14030378]
32. Tummino, M.L.; Laurenti, E.; Bracco, P.; Cecone, C.; Parola, V.L.; Vineis, C.; Testa, M.L. Antibacterial properties of functionalized cellulose extracted from deproteinized soybean hulls. Cellulose; 2023; 30, pp. 7805-7824. [DOI: https://dx.doi.org/10.1007/s10570-023-05339-w]
33. Testa, M.L.; Pandoli, O.G.; Cecone, C.; Laurenti, E.; La Parola, V.; Vineis, C.; Tummino, M.L. Sustainable Grafting of (Ligno)Cellulose-Based Powders with Antibacterial Functionalities: Effect of Biomass Type and Synthesis Conditions. Advanced Sustain. Syst.; 2024; 2400710. [DOI: https://dx.doi.org/10.1002/adsu.202400710]
34.
35.
36. Marmur, A. A guide to the equilibrium contact angles maze. Contact Angle Wettability and Adhesion; K.L. Mittal: Leiden, The Netherlands, 2009; Volume 6, 3.
37.
38.
39.
40. Hughes, A.E.; Easton, C.D.; Gengenbach, T.R.; Biesinger, M.C.; Laleh, M. Interpretation of complex x-ray photoelectron peak shapes. I. Case study of Fe 2p3/2 spectra. J. Vac. Sci. Technol. A; 2024; 42, 053205. [DOI: https://dx.doi.org/10.1116/6.0003804]
41. Videira-Quintela, D.; Guillen, F.; Martin, O.; Cumbal, L.; Montalvo, G. Antibacterial and antioxidant triple-side filler composed of fumed silica, iron, and tea polyphenols for active food packaging. Food Control; 2022; 138, 109036. [DOI: https://dx.doi.org/10.1016/j.foodcont.2022.109036]
42. Armijo, L.M.; Wawrzyniec, S.J.; Kopciuch, M.; Brandt, Y.I.; Rivera, A.C.; Withers, N.J.; Cook, N.C.; Huber, D.L.; Monson, T.C.; Smyth, H.D.C. et al. Antibacterial activity of iron oxide, iron nitride, and tobramycin conjugated nanoparticles against Pseudomonas aeruginosa biofilms. J. Nanobiotechnol.; 2020; 18, 35. [DOI: https://dx.doi.org/10.1186/s12951-020-0588-6] [PubMed: https://www.ncbi.nlm.nih.gov/pubmed/32070354]
43. Gholami, A.; Mohammadi, F.; Ghasemi, Y.; Omidifar, N.; Ebrahiminezhad, A. Antibacterial activity of SPIONs versus ferrous and ferric ions under aerobic and anaerobic conditions: A preliminary mechanism study. IET Nanobiotechnol.; 2020; 14, pp. 155-160. [DOI: https://dx.doi.org/10.1049/iet-nbt.2019.0266] [PubMed: https://www.ncbi.nlm.nih.gov/pubmed/32433033]
44. Kim, H.-E.; Lee, H.-J.; Kim, M.S.; Kim, T.; Lee, H.; Kim, H.-H.; Cho, M.; Hong, S.-W.; Lee, C. Differential Microbicidal Effects of Bimetallic Iron–Copper Nanoparticles on Escherichia coli and MS2 Coliphage. Environ. Sci. Technol.; 2019; 53, pp. 2679-2687. [DOI: https://dx.doi.org/10.1021/acs.est.8b06077]
45. Kokkarachedu, V.; Chandrasekaran, K.; Sisubalan, N.; Jayaramudu, T.; Vijayan, A.; Sadiku, R. SiO2-Based Nanomaterials as Antibacterial and Antiviral Agents: Potential Applications. Nanoparticles in Modern Antimicrobial and Antiviral Applications; Kokkarachedu, V.; Sadiku, R. Springer International Publishing: Cham, Switzerland, 2024; pp. 65-95.
46. Saravanan, P.; Duraibabu, D.; Jayamoorthy, K.; Suresh, S.; Kumar, S.A. Twin Applications of Tetra-Functional Epoxy Monomers for Anticorrosion and Antifouling Studies. Silicon; 2018; 10, pp. 555-565. [DOI: https://dx.doi.org/10.1007/s12633-016-9489-6]
47. Pistone, A.; Scolaro, C.; Visco, A. Mechanical Properties of Protective Coatings against Marine Fouling: A Review. Polymers; 2021; 13, 173. [DOI: https://dx.doi.org/10.3390/polym13020173]
You have requested "on-the-fly" machine translation of selected content from our databases. This functionality is provided solely for your convenience and is in no way intended to replace human translation. Show full disclaimer
Neither ProQuest nor its licensors make any representations or warranties with respect to the translations. The translations are automatically generated "AS IS" and "AS AVAILABLE" and are not retained in our systems. PROQUEST AND ITS LICENSORS SPECIFICALLY DISCLAIM ANY AND ALL EXPRESS OR IMPLIED WARRANTIES, INCLUDING WITHOUT LIMITATION, ANY WARRANTIES FOR AVAILABILITY, ACCURACY, TIMELINESS, COMPLETENESS, NON-INFRINGMENT, MERCHANTABILITY OR FITNESS FOR A PARTICULAR PURPOSE. Your use of the translations is subject to all use restrictions contained in your Electronic Products License Agreement and by using the translation functionality you agree to forgo any and all claims against ProQuest or its licensors for your use of the translation functionality and any output derived there from. Hide full disclaimer
© 2025 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license (https://creativecommons.org/licenses/by/4.0/). Notwithstanding the ProQuest Terms and Conditions, you may use this content in accordance with the terms of the License.
Abstract
The development of eco-friendly paint formulations is part of the transition process to more sustainable materials, which involves many industries such as offshore and shipbuilding, where the deterioration of steel in seawater is a key factor. This article aims to produce innovative coatings and test their protective action on DH 36 steel plates. SiO2 and TiO2 were modified with amino groups and iron sites to be used as filler for the design of ecological paint formulations The antimicrobial features of both NH2 groups and iron ionic species were combined with the chemical and mechanical stability of silica and titania, with silica-based powders showing increased efficacy. The surface properties of the resulting coatings were examined by determination of thickness, water wettability, roughness, and cross-cut adhesion tests (before and after a degradation test in seawater according to ASTM D870-97 standards). Preliminary tests of the microbiological activity of the iron amino functionalized materials were carried out to monitor, as proof of concept, the growth of some bacterial strains through measurements of optical density. The findings indicate that these coatings not only provide effective corrosion protection but are promising for enhancing the durability and environmental performance of steel surfaces exposed to marine environments.
You have requested "on-the-fly" machine translation of selected content from our databases. This functionality is provided solely for your convenience and is in no way intended to replace human translation. Show full disclaimer
Neither ProQuest nor its licensors make any representations or warranties with respect to the translations. The translations are automatically generated "AS IS" and "AS AVAILABLE" and are not retained in our systems. PROQUEST AND ITS LICENSORS SPECIFICALLY DISCLAIM ANY AND ALL EXPRESS OR IMPLIED WARRANTIES, INCLUDING WITHOUT LIMITATION, ANY WARRANTIES FOR AVAILABILITY, ACCURACY, TIMELINESS, COMPLETENESS, NON-INFRINGMENT, MERCHANTABILITY OR FITNESS FOR A PARTICULAR PURPOSE. Your use of the translations is subject to all use restrictions contained in your Electronic Products License Agreement and by using the translation functionality you agree to forgo any and all claims against ProQuest or its licensors for your use of the translation functionality and any output derived there from. Hide full disclaimer
Details







1 Institute for the Study of Nanostructured Materials (ISMN)—CNR, via Ugo La Malfa, 153, 90146 Palermo, Italy;
2 Department of Engineering, University of Messina, C. da Di Dio, 98166 Messina, Italy
3 Department of Engineering, University of Messina, C. da Di Dio, 98166 Messina, Italy; Institute for Polymers, Composites and Biomaterials—CNR IPCB, Via Paolo Gaifami 18, 95126 Catania, Italy
4 IRBIM-CNR, Spianata San Rainieri, 86, 98122 Messina, Italy;