ARTICLE
Received 4 Dec 2014 | Accepted 15 Jun 2015 | Published 23 Jul 2015
Jeong-Gyu Song1, Gyeong Hee Ryu2, Su Jeong Lee3, Sangwan Sim1, Chang Wan Lee1, Taejin Choi1, Hanearl Jung1, Youngjun Kim1, Zonghoon Lee2, Jae-Min Myoung3, Christian Dussarrat4, Clement Lansalot-Matras5,Jusang Park1, Hyunyong Choi1 & Hyungjun Kim1
The effective synthesis of two-dimensional transition metal dichalcogenides alloy is essential for successful application in electronic and optical devices based on a tunable band gap. Here we show a synthesis process for Mo1 xWxS2 alloy using sulfurization of super-cycle atomic layer deposition Mo1 xWxOy. Various spectroscopic and microscopic results indicate that the synthesized Mo1 xWxS2 alloys have complete mixing of Mo and W atoms and tunable band gap by systematically controlled composition and layer number. Based on this, we synthesize a vertically composition-controlled (VCC) Mo1 xWxS2 multilayer using ve continuous super-cycles with different cycle ratios for each super-cycle. Angle-resolved X-ray photo-emission spectroscopy, Raman and ultravioletvisible spectrophotometer results reveal that a VCC Mo1 xWxS2 multilayer has different vertical composition and broadband light absorption with strong interlayer coupling within a VCC Mo1 xWxS2 multilayer. Further, we demonstrate that a VCC Mo1 xWxS2 multilayer photodetector generates three to four times greater photocurrent than MoS2- and WS2-based devices, owing to the broadband light absorption.
1 School of Electrical and Electronic Engineering, Yonsei University, Seoul 120-749, Korea. 2 School of Materials Science and Engineering, Ulsan National Institute of Science and Technology (UNIST), Ulsan 689-798, Korea. 3 Department of Materials Science and Engineering, Yonsei University, Seoul 120-749, Korea. 4 Air Liquide Laboratories, Wadai 28, Tsukuba, Ibaraki 300-4247, Japan. 5 Air Liquide Laboratories Korea, Yonsei Engineering Research Park,50 Yonsei-ro, Seodaemun-gu, Seoul 120-749, Korea. Correspondence and requests for materials should be addressed to H.K. (email: mailto:[email protected]
Web End [email protected] ).
NATURE COMMUNICATIONS | 6:7817 | DOI: 10.1038/ncomms8817 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications 1
& 2015 Macmillan Publishers Limited. All rights reserved.
DOI: 10.1038/ncomms8817 OPEN
Controllable synthesis of molybdenum tungsten disulde alloy for vertically composition-controlled multilayer
ARTICLE NATURE COMMUNICATIONS | DOI: 10.1038/ncomms8817
The band gap modulation of two-dimensional (2D) transition metal dichalcogenides (TMDCs) has been intensively studied, because of their various applications
in optoelectronic devices such as photodiodes, phototransistors and solar cells13. It is well known that the band gap of 2D TMDCs is dependent on the number of layers46. In addition, alloying 2D TMDCs through the synthesis of Mo1 xWxS2,
Mo1 xWxSe2 or MoS2xSe2(1 x), for example, is another way
of practically modulating the band gap. This is an effective approach because of the good thermodynamic stability at room temperature of the alloys, as predicted by theoretical calculations714. Furthermore, recent studies have shown that a vertically composition-controlled (VCC) 2D TMDCs multilayer is feasible for the high performance optoelectronic devices due to functionality of interlayer such as interlayer transition1522. However, the reported synthesis processes for 2D TMDCs alloy and VCC 2D TMDCs multilayer, such as exfoliation, chemical vapor deposition and transfer, are limited in respect of systematic control of the composition and the number of layers, and clean interface for strong interlayer coupling9,11,21,23. Hence, an improved synthesis process for 2D TMDCs alloy and VCC 2D TMDCs multilayer is highly required.
Atomic layer deposition (ALD), which is based on surface reactions between precursors and reactants, has benets such as high purity, thickness control on the atomic scale and large area uniformity24,25. In particular, it is suitable for the synthesis of alloy thin lms with precisely controlled composition using the super-cycle method2628. In addition, a continuous super-cycle process with different cycle ratios can produce a VCC multilayer with a clean interface29. In a previous report, we have shown that atomically thin, layer-controlled and wafer-level uniform 2D WS2 can be synthesized by sulfurization of ALD WO3 thin lms30.
Here we report a synthesis method of Mo1 xWxS2 alloys by
sulfurization of super-cycle ALD Mo1 xWxOy alloy thin lms.
Using this method, we systematically control the composition and layer number (from mono- to tri-layers) of Mo1 xWxS2 alloys by
controlling the cycle ratio between the ALD MoOx and WO3. The bandgaps of the Mo1 xWxS2 alloys are precisely controlled as
functions of the composition and layer numbers of each respective alloy, as measured based on the photoluminescence (PL) spectra. Scanning transmission electron microscopy (STEM) shows the mixing of Mo and W atoms with shared metal atom sites in monolayer Mo1 xWxS2 alloy. Furthermore, we develop a
process to synthesize a VCC Mo1 xWxS2 multilayer using a
sequential super-cycle ALD processspecically, 5 continuous super-cycles of ALD with different cycle ratios for each super-cycle. Ultravioletvisible spectrophotometer analysis shows that the synthesized VCC Mo1 xWxS2 multilayer has stronger
interlayer coupling than that of a stacked VCC Mo1 xWxS2 multilayer fabricated by the individual transfer of each monolayer
Mo1 xWxS2 alloy. This can be attributed to the clean interface
between each layer in the synthesized sample15,21.
ResultsMoS2 synthesis. Previously, we reported the synthesis of WS2 using sulfurization of ALD WO3 thin lm with a one-step sulfurization process at 1,000 C (ref. 30). These synthesized WS2 exhibit smooth and continuous surfaces with layer controllability from mono- to tetra-layer. Based on this result, we sulfurized ALD MoOx thin lm (nine cycles, optimization of ALD MoOx is represented in Supplementary Fig. 1) using a one-step sulfurization process at 1,000 C (see experimental section) to synthesize MoS2. Figure 1a,b comprises scanning electron microscope (SEM) and atomic force microscopy (AFM) images of sulfurized MoOx thin lm using the one-step sulfurization
process at 1,000 C. In contrast to WS2, however, the MoS2 shows a rough and non-continuous surface, and the measured root mean square (r.m.s.) is much larger (1.4 nm) than that of the SiO2 substrate (0.37 nm). We surmise that this discrepancy between the MoOx and WO3 thin lms sulfurized at the same temperature (1,000 C) is caused by the relatively lower vaporization temperature of MoOx (B700 C) in comparison with WO3 (over 1,100 C)31. In other words, the MoOx is vaporized before the conversion to MoS2 is complete, resulting in a rough surface.
Therefore, we examined the effect of sulfurization temperature on the roughness of the sulfurized ALD MoOx thin lm. To achieve this, we conducted a two-step sulfurization process, which consists of a low-temperature rst step for the sulfurization of the MoOx and a high-temperature second step to enhance the MoS2 crystallinity. The rst-sulfurization temperatures were set to lower (600 C) and higher (800 C) temperatures than the vaporization temperature of MoOx (700 C), while the second-sulfurization temperature and process time were kept at 1,000 C and 150 min, respectively (see Methods section). The roughness of the sulfurized MoOx thin lms in accordance with rstsulfurization temperature was then compared using SEM and AFM (Fig. 1cf). Figure 1c,e shows SEM images of the sulfurized MoOx thin lms for rst-sulfurization temperatures of 600 C and 800 C, respectively. The sulfurized MoOx thin lm at a rst-sulfurization temperature of 600 C has a smooth and continuous surface, while the MoOx thin lm sulfurized at a rst-sulfurization temperature of 800 C has a rough and
One step 1,000 C
One step1,000 C, r.m.s. = 1.4 nm
Two step 600 C
Two step600 C, r.m.s. = 0.4 nm
Two step 800 C
Two step800 C, r.m.s. = 0.8 nm
Figure 1 | Sulfurization of MoOx thin lms. (a) SEM and (b) AFM images of sulfurized MoOx thin lm using one-step sulfurization process at 1,000 C. SEM and AFM images of sulfurized MoOx thin lm using two-step sulfurization process with rst-sulfurization temperatures of (c,d) 600 and (e,f) 800 C, respectively. Scale bars, (a,c,e) 200 nmand (b,d,f) 0.5 mm.
2 NATURE COMMUNICATIONS | 6:7817 | DOI: 10.1038/ncomms8817 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications
& 2015 Macmillan Publishers Limited. All rights reserved.
NATURE COMMUNICATIONS | DOI: 10.1038/ncomms8817 ARTICLE
non-continuous surface. AFM analyses (Fig. 1d,f) illustrate the variations in the roughness of the sulfurized MoOx thin lms more clearly, which is due to the differing rst-sulfurization temperatures. The r.m.s. value for the MoS2 sulfurized at 600 C is very low (B0.4 nm) and is close to the r.m.s. value of the SiO2 substrate (0.37 nm). In contrast, the r.m.s. value of the MoS2 in
the 800 C case is relatively high (0.8 nm). As a result, a rstsulfurization temperature of 600 C results in MoS2 with uniform and continuous surfaces, due to the fact that the rst-sulfurization temperature is lower than the vaporization temperature of MoOx,
as we assumed. Based on this result, we used a two-step sulfurization process with a 600 C rst-sulfurization temperature to synthesize continuous MoS2 and Mo1 xWxS2 alloys.
Next, layer-number-controlled MoS2 was synthesized utilizing the two-step sulfurization process described above. Figure 2ad shows the AFM images and height proles of the transferred MoS2, which were synthesized by sulfurizing MoOx thin lms deposited by 6, 9 and 12 ALD cycles. The measured thicknesses of the synthesized MoS2 were B1, 1.6 and 2.3 nm for 6, 9 and 12
MoOx ALD cycles, respectively. These thicknesses correspond to mono-, bi- and tri-layer (1, 2 and 3l) MoS2, considering that the height of 1l MoS2 on SiO2 is B1 nm and the spacing between the rst and second MoS2 layers is B0.6 nm (refs 3,4). As reported previously, the larger AFM-measured spacing between the rst MoS2 layer and the substrate, compared with that between the
MoS2 layers, is caused by the effect of distinct tipsample and tipsubstrate interactions3,30,32. Also, the apparent colour gains of the transferred 1, 2 and 3l MoS2 are observed in optical microscopy (OM) images (Supplementary Fig. 2). It should be noted that the MoS2 is not formed in the case of an ALD MoOx thin lm with an ALD cycle number of o3 (Supplementary
Fig. 3). This is attributed to a nucleation delay during the initial growth of the MoOx, and similar behaviour was observed during the synthesis of WS2 by sulfurization of ALD WO3 (ref. 30). After the nucleation delay, 1l of MoS2 is formed by the sulfurization of each three-cycle ALD MoOx thin lm sample (B0.8 0.9 nm in
thickness). This observation agrees with a previous report, where
B1 nm of MoOx lm transformed into a 1l MoS2 via sulfurization33. The stoichiometry calculated from X-ray photoemission spectroscopy (XPS) result is 2 (S/Mo) as shown in Supplementary Fig. 4. As a result, we can systematically control the layer number of MoS2 by controlling the ALD MoOx cycle number.
The MoS2 were further characterized using Raman, PL and high-resolution TEM (HRTEM). The Raman spectra (lexc 532 nm) for 1, 2l and 3l MoS2 are shown in Fig. 2e. The
MoS2 exhibit in-plane and out-of-plane vibrations modes at 386.6 and 406.5 cm 1 (E0 and A01) for the 1l, 385.6 and 407.6 cm 1 (Eg1 and A1g) for 2l, and 384.7 and 408.5 cm 1 (E01 and A01) for 3l (ref. 34). From the Raman spectra, we calculated the relative peak distance between the in-plane and out-of-plane modes, which is closely related to the layer number of the MoS2 due to the softening in the in-plane and stiffening in the out-of-plane mode frequencies, with increasing layer numbers35,36. The calculated relative peak distances are 19.9, 22 and 23.8 cm 1 for the 1, 2 and 3l samples, respectively, which are in good agreement with previously reported values for synthesized MoS2 (refs 3739).
The PL spectra dependence on the layer number of the MoS2 is
shown in Fig. 2f. The spectrum of the 1l MoS2 shows PL peaks at1.89 eV and 2.01 eV, which are correlated to the A1 and B1 direct excitonic transitions of the MoS2, respectively. With increasing layer number, weak PL peaks are observed at 1.87 eV and 2.00 eV for the 2l, and 1.86 eV and 1.99 eV for the 3l. The red shift and low intensity of the PL peaks with increasing layer number is due to the band gap transition from direct to indirect, which is consistent with the dependency of the PL peak on the layer number46,40. These Raman and PL results again conrm the layer controllability of MoS2 using the ALD process. Figure 2g is an HRTEM image for the synthesized 1l MoS2. The MoS2 shows a honeycomb-like structure with lattice spacing of 0.27 nm and0.16 nm for the (100) and (110) planes, respectively. In addition, sixfold coordination symmetry is observed in the fast Fourier transformation (FFT) image (inset of Fig. 2g). The approximate
1L 2L 3L
16 1L 1 nm
1.6 nm
Height (nm)
2L
4 3L 2.3 nm
0 0.3
0.6
A
1
Position (m)
E
386.6 406.5
407.6
1L
A1g
Intensity (a.u.)
Eg1
1L
385.6
384.7 408.5
PL intensity (a.u.)
2L
(100)2.7
A
1
2L
E1
(110)1.6
3L
3L
350 450
400 1.8 1.5
Raman shift (cm1)
2.1
Energy (eV)
Figure 2 | Characterization of MoS2. (ac) AFM images and (d) height proles (along with white dashed line in AFM images) of transferred MoS2on SiO2 substrate for 1l, 2l and 3l thickness, respectively. Scale bars, 0.5 mm. (e) Raman spectra and (f) PL spectra for 1l (red), 2l (blue) and 3l (black)
MoS2 on SiO2 substrate. (g) HRTEM image of 1l MoS2 at a selected region and (inset) FFT pattern. Scale bars, 2 nm.
NATURE COMMUNICATIONS | 6:7817 | DOI: 10.1038/ncomms8817 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications 3
& 2015 Macmillan Publishers Limited. All rights reserved.
ARTICLE NATURE COMMUNICATIONS | DOI: 10.1038/ncomms8817
domain size is 10 20 nm, similar to that of previously reported
synthesized MoS2 and WS2 using the sulfurization of MoOx and WO3 thin lms30,41.
Mo1 xWxS2 alloy synthesis. A super-cycle ALD-based
Mo1 xWxS2 alloy synthesis process was developed based on the
synthesis processes for 2D MoS2 (this study) and WS2 (previous study)30. The overall synthesis scheme for the Mo1 xWxS2 alloy
is illustrated in Fig. 3a. First, we conducted 10 cycles of WO3 ALD to address the nucleation delay of the ALD WO3 (ref. 30) (not shown in Fig. 3a). Subsequently, one super-cycle ALD process consisting of n cycles of ALD MoOx and m cycles of ALD WO3 was conducted and the deposited Mo1 xWxOy alloy thin lms
were sulfurized. We used varying cycles for MoOx (n) and
WO3 (m) in one super-cycle to deposit 0.8 0.9-nm-thick
composition-controlled Mo1 xWxOy alloy thin lms to create a
1l Mo1 xWxS2 alloy. This was based on the growth rate of ALD
MoOx (2.7 per cycle) and WO3 (0.9 per cycle), as shown in Supplementary Table 1. Figure 3bd shows the XPS spectra of the 1l MoS2, 1l WS2 and sulfurized Mo1 xWxOy alloy thin lms with
different n and m numbers in one super-cycle. All measured XPS results were normalized by S2p3/2 peak intensity and calibrated to the C1s peak at 285 eV. With increasing n/m ratio, the intensity of the Mo3d peaks increased, while the W5p3/2 and W4f peaks
decreased. Furthermore, the peak positions for Mo3d and W4f gradually shifted to higher binding energies, from 232.2 eV and 229.1 eV to 232.5 eV and 229.4 eV for Mo3d3/2 and Mo3d5/2,
respectively, and from 34.8 eV and 32.6 eV to 35.0 eV and 32.8 eV for W4f5/2 and W4f7/2, respectively. In addition, the S2p peaks shifted to lower binding energies, from 163.5 eV and 162.4 eV to 163.3 eV and 162.2 eV for S2p1/2 and S2p3/2, respectively. This small shift in peak position is attributed to the enhanced electron attraction strength of S and the reduced electron attraction strength of W, following increased Mo content due to smaller electronegativity of Mo (2.16) than that of W (2.36) as previously reported7. It is noteworthy that the Mo6 3d3/2 peak, which is attributed to the MoO bonding, is not observed in the Mo3d spectra; this indicates the absence of O species.
We calculated the Mo, W and S concentrations from the XPS results for the Mo3d, W4f and S2p peaks, respectively, to examine the Mo1 xWxS2 alloy composition. Table 1 presents the
calculated concentration and W composition, x. The calculated x value is dependent on the n and m numbers in a single super-cycle, and yields x 0.8 for n 1 and m 6, x 0.6 for n 2 and
m 4, and x 0.3 for n 3 and m 1. Also, the calculated
stoichiometry is 2 (S/(Mo W)). This shows that the W
composition (x) in the Mo1 xWxS2 alloys can be systematically
modulated by changing the values of n and m in one super-cycle.
The synthesized composition-controlled Mo1 xWxS2 alloy from super-cycle ALD Mo1 xWxOy alloy thin lms were
characterized using AFM, Raman and PL, as shown in Fig. 4. The AFM images and height proles of the transferred Mo1 xWxS2 alloys are represented in Fig. 4a d and they
show good uniformity and continuity (also see OM images in
ALD MoOx n cycles
ALD WO3 m cycles
One super-cycle ALD
Mo1xWxOy Mo1xWxS2
Mo3d
W4f
S2p
4f5/2
4f7/2
2p1/2
2p3/2
3d3/2 3d5/2 S2s
WS2
5p3/2
WS2
Normalized intensity (a.u.)
WS2
n=1 m=6
n=2 m=4
n=3 m=1
MoS2
n=1 m=6
n=2
m=4
n=3 m=1
MoS2
n=1 m=6
n=2
m=4
n=3 m=1
MoS2
235 230 225 40
Binding energy (eV)
35 30 165 162 159
Figure 3 | Synthesis and XPS of Mo1 xWxS2 alloy. (a) Synthesis procedure of super-cycle ALD for Mo1 xWxS2 alloy. XPS measurements for
(b) Mo3d, (c) W4f and (d) S2p core levels in the 1l Mo1 xWxS2 alloy with different n and m numbers in one super-cycle. All measured XPS results
are normalized by S2p3/2 peak intensity.
4 NATURE COMMUNICATIONS | 6:7817 | DOI: 10.1038/ncomms8817 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications
& 2015 Macmillan Publishers Limited. All rights reserved.
NATURE COMMUNICATIONS | DOI: 10.1038/ncomms8817 ARTICLE
Supplementary Fig. 5). The measured thicknesses of the Mo0.2W0.8S2, Mo0.4W0.6S2 and Mo0.7W0.3S2 alloys were all
B1 nm, corresponding to the 1l thickness of Mo1 xWxS2 alloy. Furthermore, 2 and 3l Mo1 xWxS2 alloys can be synthesized
using two- and three-super-cycle ALD Mo1 xWxOy alloy thin
lms (Supplementary Fig. 6). As a result, our super-cycle ALD-based Mo1 xWxS2 alloy synthesis process can systematically
control the layer number, as well as the composition of the resultant alloys through manipulation of the super-cycle ALD process.
Figure 4e shows the Raman spectra of composition-controlled 1l Mo1 xWxS2 alloys. The 1l WS2 (x 1) exhibits rst-order
modes: out-of-plane (A01) and in-plane (E0) modes at 417 cm 1 and 357 cm 1, respectively, and a second-order mode: 2LA(M)
at 353 cm 1 (ref. 30). The A01 mode shifts to a lower frequency with decreasing W composition, while the E0 mode related to WS2 does not noticeably shift with the reduction of intensity. In addition, an E0 mode related to MoS2 appear at x 0.8 and
shifted to a higher frequency with a reduction in W composition. The specic peak position dependency on W composition is represented in Supplementary Fig. 7, and the W composition
dependence of the Raman spectra of the 1l Mo1 xWxS2 alloy is
consistent with previous reports79.
The normalized PL spectra of the composition-controlled 1l Mo1 xWxS2 alloys are shown in Fig. 4f, also the x values versus
the average PL peak positions and s.d. of ve-times repeatedly synthesized 1l Mo1 xWxS2 alloys are plotted in Fig. 4g. As the
value of x increased from 0 to 1, the averaged PL peak position initially decreases from 1.885 to 1.863 eV, and then gradually increases to 2.021 eV. This non-linear PL peak position behaviour with changing x is the so-called bowing effect, and has also been reported for other semiconducting alloys and exfoliated 1l Mo1 xWxS2 alloys9,42,43. The bowing effect in 1l Mo1 xWxS2
alloy can be described by the Equation (1),
EPL;Mo1 xWxS2 1 x
EPL;MoS2 xEPL;WS2 bx1 x; 1
where b is a bowing parameter. After tting the experimental results as shown in Fig. 4g (red solid curve), a b value of0.250.03 eV was extracted. The extracted b value is comparable to that of the previous experiment (0.250.04 eV) and simulation (0.280.04 eV) results9. Furthermore, the s.d. of the ve-times repeatedly synthesized 1l Mo1 xWxS2 alloys are small
within the range of 0.008 to 0.01, which indicates that the process has good reliability in terms of composition control. Thus, the PL result conrms that we modulate the band gap of the Mo1 xWxS2 alloy by reliably controlling the composition.
Moreover, the band gap can also be modulated by controlling the layer number (see Supplementary Fig. 8).
Figure 5a is the HRTEM image of the 1l Mo0.4W0.6S2
alloy (x 0.6). The Mo0.4W0.6S2 alloy shows a periodic atomic
arrangement with a honeycomb-like structure and sixfold coordination symmetry, similar to the 1l MoS2 shown in
Fig. 2f. To distinguish between the W and Mo atoms in the 1l Mo0.4W0.6S2 alloy, we analysed the Mo0.4W0.6S2 alloy using STEM
Table 1 | Calculated composition of Mo1 xWxS2.
One super-cycle Mo (%) W (%) S (%) W composition x n m1 6 6.9 26.5 66.6 0.82 4 12.5 19.3 68.2 0.63 1 22.5 10.5 67 0.3
Quantication analysis for Mo3d, W4f and S2p peaks depending on n and m number in one super-cycle. The calculation error for the composition is under 1%.
x=0.8 1L x=0.3 1L
x=0.6 1L
x=0.8
x=0.6
x=0.3
1 nm
1 nm
1 nm
Height (nm)
16
12
8
4
0 0.3 0.6 Position (m)
E (WS2)
A1
x=1
Intensity (a.u.)
Normalized PL intensity (a.u.)
Emission peak position (eV)
2.0
x=0.8
x=1
x=0.8
b=0.25 0.03 eV
x=0.6
x=0.6
x=0.3
x=0.3
x=0
x=0
300
E (MoS2)
0.0 0.5 1.0
Figure 4 | Characterization of Mo1 xWxS2 alloy. (ac) AFM images and (d) height proles (along with white dashed line in AFM images) of transferred 1l
Mo1 xWxS2 alloy on SiO2 substrate for x 0.8, 0.6 and 0.3, respectively. Scale bars, 0.5 mm. (e) Raman spectra and (f) PL spectra for 1l Mo1
xWxS2
400
Raman shift (cm1) Energy (eV)
500 2.0
1.9
1.8
W composition x
alloy on SiO2 substrate for x 1, 0.8, 0.6, 0.3 and 0. (g) PL peak position versus W composition (x) graph. Error bars represent s.d. of PL peak position in
ve-times repeatedly synthesized Mo1 xWxS2 alloy.
NATURE COMMUNICATIONS | 6:7817 | DOI: 10.1038/ncomms8817 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications 5
& 2015 Macmillan Publishers Limited. All rights reserved.
ARTICLE NATURE COMMUNICATIONS | DOI: 10.1038/ncomms8817
annular dark-eld and energy dispersive X-ray spectrometry (EDX). Figure 5b is the STEM-ADF image of the 1l Mo0.4W0.6S2
alloy. Brighter and less bright spots, which correspond to W and Mo atoms, respectively, are clearly resolved in the ADF image, as previously reported44. The calculated Mo/W ratio from the atom count in Fig. 5b is 0.42:0.58, which differs by o5% from the
XPS-measured stoichiometry. In addition, the EDX result in Fig. 5c supports the presence of W, Mo and S species in the 1l Mo0.4W0.6S2 alloy. To extract a clear intensity difference between the W and Mo atoms, we performed an inverse FFT by applying a mask to the yellow dashed square region in Fig. 5b. Figure 5de shows the inversed FFT image (Fig. 5d) and intensity prole (Fig. 5e) along with the yellow solid line in Fig. 5d. Although S atoms are not distinguishable in our result as a result of the displacement of S atoms at 200 kV operation voltage by the knock-on mechanism45, the W and Mo atoms are clearly observable, conrming that these elements share the metal atom sites44. The preference for Mo or W atoms at the neighbouring sites of W atoms is evaluated by degree of alloying that can be calculated by Equation (2)23,44,
JW P
observed=Prandom 100%; 2
where Pobserved is the averaged ratio of number of neighbouring
Mo atoms to total neighbouring sites of W atoms, and Prandom is
the total ratio of Mo atoms in the examined layer. Figure 5f represented differently coloured W atoms depending on number of neighbouring Mo atoms: light brown, blue, red, dark red, yellow, green and violet for six, ve, four, three, two, one and zero number of neighbouring Mo atoms. The calculated degree of alloying is 99%, which indicate that there is no preference for Mo or W atoms at the neighbouring sites of W atoms and a random mixture of our 1l Mo1 xWxS2 alloy.
A VCC Mo1 xWxS2 synthesis. The composition controllability
of our ALD-based Mo1 xWxS2 alloy synthesis process enables
synthesis of a VCC Mo1 xWxS2 multilayer with a clean interface,
strong interlayer coupling and broadband light absorption. We sulfurized a VCC Mo1 xWxOy thin lm that was deposited by a
sequential super-cycle ALD process, so as to synthesize a VCC Mo1 xWxS2 multilayer, as shown in Fig. 6a. First, we conducted
20 cycles of WO3 ALD on a SiO2 substrate, corresponding to 1l WS2. We immediately performed three super-cycles of
Mo1 xWxOy ALD with different super-cycle n and m numbers,
in the following order: n 1 and m 6, n 2 and m 4, and
n 3 and m 1. Last, we conducted three cycles of MoOx
ALD (n 3) corresponding to 1l MoS2. The deposited VCC
Mo1 xWxOy thin lm was sulfurized to convert it into a VCC
Mo1 xWxS2 multilayer. Figure 6b,c shows an AFM image and
height prole of the transferred VCC Mo1 xWxS2 multilayer,
with a measured thickness of B3.5 nm. This thickness, synthesized by ve sequential ALD super-cycles, corresponds to a 5l Mo1 xWxS2 alloy, which is consistent with each super-cycle
result for the 1l Mo1 xWxS2 alloy.
The different composition concentrations of the bottom and top layers in the VCC Mo1 xWxS2 multilayer were analysed
using angle-resolved XPS (ARXPS). Figure 6d shows the calculated atomic and relative concentration ratios of the Mo and W from the ARXPS measurement (ARXPS spectra are shown in Supplementary Fig. 9). The Mo concentration increased from18.6 to 20.9%, while the W concentration decreased from 15.7 to13.5%, with increasing emission angle from 0 to 70 (red line). The Mo/W concentration ratio increased from 1.17 to 1.55 with increasing emission angle (blue line). Although the exact atomic concentration according to position in the VCC Mo1 xWxS2 multilayer cannot be calculated because of the larger depth resolution of the XPS measurement in comparison with the VCC Mo1 xWxS2 multilayer thickness, the emission angle dependency
of the Mo and W concentration indicates Mo-rich and W-rich concentration in the upper and lower layers of the VCC Mo1 xWxS2 multilayer, respectively. As a result, ARXPS shows
that the VCC Mo1 xWxS2 multilayer has VCC characteristics.
Notably, the calculated stoichiometry ratio was 2 (S/(Mo W))
in all ARXPS results.The formation of Mo1 xWxS2 alloy with different composi
tions in a VCC Mo1 xWxS2 multilayer was analysed using
Raman spectroscopy. Figure 6e shows the Raman spectrum of a VCC Mo1 xWxS2 multilayer, which exhibits strong peaks for
A1g, MoS2-like E12g and WS2-like E12g 2LA(M) modes. Each
Raman peak can be tted using a Lorentzian function to the Raman spectrum of the Mo1 xWxS2 alloy with x 0, 0.3, 0.6,
0.8 and 1. The tted Raman spectrum was compared with the measured Raman spectrum for the 1l Mo1 xWxS2 alloy, with respect to variations in the peak position and peak distances of the A1g and MoS2-like E12g modes, depending on
W-5Mo
W-4Mo
W M
Mo L
S k
Cu k
W
W
C k
Counts (a.u.)
W-6Mo
Cu k
Intensity (a.u.)
Mo
W-3Mo W-0Mo
W-2Mo
W-1Mo
Mo
Mo
Cu L
W L
W L
Mo K
0 4 8 12 16 20 Energy (keV)
0.0 0.5 1.0
Position (nm)
Figure 5 | Atomic arrangement and mixture of Mo0.4W0.6S2 alloy. (a) HRTEM image of 1l Mo0.4W0.6S2 alloy at a selected region, and (inset) FFT pattern. Scale bars, 2 nm. (b) STEM-ADF image of 1l Mo0.4W0.6S2 alloy at a selected region and (c) corresponding EDX spectrum. Scale bars, 1 nm.
(d) Inverse FFT image with masking applied to yellow dashed square region in b. Scale bars, 1 nm. (e) Intensity prole of yellow solid line in d. (f) Coloured W atoms with light brown, blue, red, dark red, yellow, green and violet for six, ve, four, three, two, one and zero number of neighbouring Mo atoms.
6 NATURE COMMUNICATIONS | 6:7817 | DOI: 10.1038/ncomms8817 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications
& 2015 Macmillan Publishers Limited. All rights reserved.
NATURE COMMUNICATIONS | DOI: 10.1038/ncomms8817 ARTICLE
With respect to the surface normal
25
15
1.6
1.4
1.2
Sequential super-cycle nm = 30/31/24/16/020
Atomic concentration (%)
Mo/W concentration ratio
20 Mo
W
Mo/W
Mo rich
W rich
Height (nm)
10
5
0
3.5 nm
0.3 0.6 0.9 1.2
Emission angle (deg)
W composition x
Intensity (a.u.)
WS2 like E12g+2LA(M)
350 400 450
MoS2 like E12g
Raman frequency (cm1)
420
380
Position (m)
A1g from fitted Raman spectrum
Fitted Raman of x=0 x=0.3 x=0.6 x=0.8 x=1
400 Peak position from 1L Mo1-xWxS2
MoS2 like E12g from fitted Raman spectrum
Peak distances (cm1)
50
40
30
20
360 0.0 0.2 0.4 0.6 0.8 1.0
10 0 10 20 30 40 50 60 70
A1g MoS2 like E12g from fitted Raman spectrum
A1 MoS2 like E from 1L Mo1xWxS2
0.0 0.2 0.4 0.6 0.8
Raman shift (cm1)
A1g
W composition x
Figure 6 | Characterization of VCC Mo1 xWxS2 multilayer. (a) Sequential super-cycle ALD procedure and schematic structure of a VCC Mo1 xWxS2
multilayer. (b) AFM image and (c) height proles (along with white dashed line in AFM image) for a VCC Mo1 xWxS2 multilayer. Scale bars, 0.5 mm.
(d) Calculated atomic concentration and relative concentration ratio of Mo and W from ARXPS measurement. (e) Raman spectra for a VCC Mo1 xWxS2 multilayer. (f) Raman peak position of A1g and MoS2-like E12g modes from tted Raman spectra (red and blue solid line) and from measured Raman spectra of 1l Mo1 xWxS2 alloy (black dashed line). (g) Calculated Raman peak distances between A1g and MoS2-like E12g modes from tted Raman spectra
(red solid line) and from measured Raman spectra of 1l Mo1 xWxS2 alloy (black dashed line).
W concentration. The A1g and MoS2-like E12g peak positions from the tted Raman spectrum are represented in Fig. 6f with the measured Raman peak positions for the 1l Mo1 xWxS2 alloy (black dashed line, the same as Supplementary Fig. 7). The variation in the tted Raman peak position with increasing W concentration in the Mo1 xWxS2 alloy is the same as the
variation in the measured Raman peak position for the 1l Mo1 xWxS2 alloy: A1g shifts to a higher frequency with an
increase in W concentration, while the MoS2-like E12g modes downshift. Figure 6g shows peak distances between the A1g and
MoS2-like E12g modes from the tted Raman spectrum (red solid line) and measured Raman spectrum of the 1l Mo1 xWxS2 alloy (black dashed line), which are 3 4 cm 1 larger than that of the
Raman spectrum of the 1l Mo1 xWxS2 alloy. This is due to the
softening in the MoS2-like E12g mode frequency and stiffening in the A1g mode frequency. Similar behaviour, that is, increasing peak distances with increasing layer number, is also observed in MoS2 (refs 35,36) and WS2 (ref. 30) because of the reduced long-range Coulomb interaction between the effective charges, which is induced by an increase in the dielectric screening. These results for the tted Raman spectra are in good agreement with the dependency of the peak positions on the W composition given by the measured Raman results, and the dependency of the peak distances on layer number in 2D TMDCs. Thus, we can conclude that the tted Raman spectra show the formation of a Mo1 xWxS2 alloy with different compositions in a VCC
Mo1 xWxS2 multilayer.
As a result, it can be stated that the ARXPS and Raman results show the VCC characteristics of a VCC Mo1 xWxS2 multilayer.
Also, these ndings indicate that the vertical interdiffusion of the Mo and W atoms during the sulfurization process have no critically effect on the VCC characteristics. A similar result was observed in a previous report, in that MoOx/WO3 thin lm was converted to MoS2/WS2 without the formation of a Mo1 xWxS2
alloy, indicating the limited interdiffusion of Mo and W atoms46.
Further, it is noteworthy that we veried the validity of ARXPS and Raman measurements as a means of characterizing the VCC Mo1 xWxS2 multilayer via characterization of a VCC
Mo1 xWxS2 multilayer synthesized with a reversed vertical
composition prole (see Supplementary Fig. 10).
Since the interlayer coupling affects interlayer transition15,21,47,48, strong interlayer coupling in a synthesized VCC Mo1 xWxS2 multilayer was evaluated using comparison of interlayer transition in three difference sample types as shown in Fig. 7a. Sample 1 is a stacked VCC Mo1 xWxS2 multilayer fabricated by the transfer of
each differently composed Mo1 xWxS2 alloy onto glass substrate,
while sample 2 is the same as sample 1 but annealed at 200 C for 15 min in an Ar ambient atmosphere to enhance the interlayer coupling by the removal of residual molecules21,48. Sample 3 is a transferred VCC Mo1 xWxS2 multilayer on glass substrate, which
was annealed at 200 C for 15 min in an Ar ambient atmosphere. Ultravioletvisible spectrophotometer measurements for samples 1, 2 and 3 (Fig. 7b) illustrate that these have broadband light absorption properties due to the sum of the light absorption from the differently composed Mo1 xWxS2 alloys. In previous reports,
the absorption spectrum of the interlayer transition could be obtained by comparing the intensity difference between the absorption spectra of the weakly interlayer-coupled sample and that of the strongly interlayer-coupled sample15,48. Based on these reports, we extracted the interlayer transition absorption spectrum by subtracting the absorption spectrum of sample 1 from that of sample 2 and of sample 3, since sample 1 has the weakest interlayer coupling of the three samples as a result of the contamination at the interface caused by the layer transfer process15,21,48. The extracted absorption spectra of the interlayer transition are shown in Fig. 7c. The sample 2sample 1 spectrum (black solid line) shows a small absorbance peak at 1.87 eV, while the sample 3sample 1 spectrum (red solid line) shows an absorbance peak that is over ve times stronger than the sample 2sample 1 absorbance peak at the same position. Specic observations on the origin of the absorbance peak
NATURE COMMUNICATIONS | 6:7817 | DOI: 10.1038/ncomms8817 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications 7
& 2015 Macmillan Publishers Limited. All rights reserved.
ARTICLE NATURE COMMUNICATIONS | DOI: 10.1038/ncomms8817
Sample 1
x=0
x=0.3
x=0.6
x=0.8
x=1
Sample 3
Sample 2 annealing @ 200C(Ar, 15 min)
Transfer
Glass
Glass
Glass
A stacked VCC Mo1xWxS2 multilayer
Annealed a stacked VCC Mo1-xWxS2 multilayer
A VCC Mo1xWxS2 multilayer
Absorption spectra
0.2
0.0
0.1
0.0
Sample 3
Sample 2
Sample 1
Absorbance
Absorption from interlayer transition
Sample 3 sample 1
Sample 2 sample 1
x8
1.6 1.7 1.8 1.9 2.0
Energy (eV)
VCC Mo1xWxS2
On On On
On On
On
VCC Mo1xWxS2
Off
Off
Off
Off
Off
Off
Off Off
Off
Off
WS2
MoS2
Photocurrent (a.u.)
I ds (nA)
2.30
2.25
2.15
2.10
2.25
2.20
On
On
WS2
MoS2
On
On
On On
Off
Off
1.2 1.5 1.8 2.1 2.4 40
30
10
20
Energy (eV)
Time (s)
Figure 7 | Absorbance and photoinduced current of VCC Mo1 xWxS2 multilayer. (a) Schematics of three sample types for ultravioletvisible
spectrophotometer measurement. (b) Absorption spectra of sample 1 (black solid line), sample 2 (blue solid line), and sample 3 (red solid line) and (c) extracted absorption spectra of interlayer transition using subtraction of sample 1 from sample 2 (black solid line) and from sample 3 (red solid line). (d) Spectral and (e) time-resolved photocurrent of a VCC Mo1 xWxS2 multilayer, 5l WS2 and 5l MoS2 photodetectors.
position from the interlayer transition (1.87 eV) are described in the Supplementary Information (Supplementary Fig. 11). The stronger absorbance peak of sample 3sample 1 in comparison with that of sample 2sample 1 indicates that sample 3 has stronger interlayer coupling compared with sample 2. In other words, a VCC Mo1 xWxS2 multilayer based on sequential super-cycle ALD has
the strongest interlayer coupling among the three types of samples. We surmise that this strong interlayer coupling results from the absence of a transfer process, which eliminates the incorporation of residual molecules such as H2O and organic contaminants15,21,47,48.
A VCC Mo1 xWxS2 multilayer exhibits a broadband light
absorption property, as well as strong interlayer coupling. Thus, the VCC Mo1 xWxS2 multilayer has promising potential use as
an active layer in an efcient photodetector. To evaluate the photoinduced response of the VCC Mo1 xWxS2 multilayer, we
observed the spectral and time-resolved photocurrent of a VCC Mo1 xWxS2 multilayer photodetector and compared it with 5l
WS2 and 5l MoS2 photodetectors (see the Methods section for details of device fabrication, and see Supplementary Fig. 12 for AFM images of the 5l MoS2 and WS2 and their IV
8 NATURE COMMUNICATIONS | 6:7817 | DOI: 10.1038/ncomms8817 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications
& 2015 Macmillan Publishers Limited. All rights reserved.
NATURE COMMUNICATIONS | DOI: 10.1038/ncomms8817 ARTICLE
characteristics). Figure 7d shows the dependence of the photo-current on the illumination energy for the VCC Mo1 xWxS2 multilayer, 5l WS2, and 5l MoS2 photodetectors for a voltage drain to source (Vds) of 5 V. The continuum power spectral density is represented in Supplementary Fig. 13. The VCC Mo1 xWxS2 multilayer photodetector generates a broadband
photoinduced current from 1.2 to 2.5 eV, because of its broadband light absorption property. In contrast, the 5l WS2 and 5l
MoS2 photodetectors generate narrower photocurrents than the VCC Mo1 xWxS2 multilayer, at 1.3 and 2.1 eV for the 5l WS2
photodetector and 1.2 and 1.8 eV for the MoS2 device; these values correspond to the 5l WS2 and MoS2 bandgaps. We then examined the time-resolved photocurrent measurement using white-light illumination, as shown in Fig. 7e (result using specic laser wavelength is shown in Supplementary Fig. 14). The white light was rst turned off for a period of 5 s, and then turned on for 5 s with the biasing Vds 5 V. The drain current (Ids) increased
on activation of the light and decayed following removal of the incident light. The induced photocurrents were 39 pA, 13 pA and 11 pA for the VCC Mo1 xWxS2 multilayer, 5l WS2 and 5l MoS2
devices, respectively. Hence, the VCC Mo1 xWxS2 multilayer
generates three to four times greater photocurrent than 5l WS2 or
5l MoS2, which is attributed to broadband light absorption. Thus, we concluded that the VCC Mo1 xWxS2 multilayer is promising
as regards use as an efcient photodetector with broadband light absorption. Furthermore, the broadband light absorption property is feasible for various optoelectronic applications such as solar cells49,50.
DiscussionIn summary, we developed an ALD-based Mo1 xWxS2 synthesis
process using sulfurization of super-cycle ALD Mo1 xWxOy thin lm. We studied the sulfurization process of ALD MoOx thin lms to produce uniform and continuous MoS2. The synthesized ALD-based Mo1 xWxS2 alloy show good stoichiometry, uniform
and continuous surfaces, controlled composition and layer numbers, and mixing of Mo and W atoms. Moreover, we developed a simple method to synthesize a VCC Mo1 xWxS2 multilayer with a clean interface, which shows stronger interlayer coupling than that of a stacked VCC Mo1 xWxS2 multilayer
fabricated using the transfer process. Further, we have shown that the VCC Mo1 xWxS2 multilayer has promising potential
applications as an efcient photodetector, because of its broadband light absorption capability. It should also be noted that the ALD-based TMDCs alloy synthesis process is not only limited to Mo1 xWxS2, and we expect that similar process strategies can be
developed for other TMDCs materials and their vertical stacks.
Methods
MoOx lm growth and characteristics. A 6-inch ALD chamber containing a loadlock chamber was used for the deposition of the MoOx lms. The lms were deposited on SiO2(300 nm)/Si substrates by plasma-enhanced ALD using Mo(CO)6 and O2 plasma at a 200 C growth temperature. The temperature of the bubbler containing Mo(CO)6 was maintained at 35 C to produce adequate vapour pressure, and vapourized Mo(CO)6 molecules were transported into the chamber by pure argon (99.999%) carrier gas. The O2 ow and plasma power were xed at 300 s.c.c.m. and 200 W, respectively. An ALD cycle consists of four steps: Mo(CO)6 precursor exposure (ts), Ar purging (tp), O2 plasma reactant exposure (tr) and another Ar purging (tp). In the ALD MoOx process, the ts, tp and tr were xed at 5 s, 12 s and 5 s, respectively. Optimization of the ALD MoOx process is described in the Supplementary Fig. 1.
Mo1 xWxOy Film Growth. MoOx and WO3 ALD processes27 were used to deposit
Mo1 xWxOy lm using super-cycle ALD (as shown in Fig. 3a) under the same
chamber and deposition conditions described above for the ALD of MoOx. After 10 cycles of WO3 ALD to address nucleation delay27, we conducted super-cycle ALD, which consists of n cycles of MoOx ALD and m cycles of WO3 ALD. The detailed process steps are shown in Supplementary Table 1.
Sulfurization processes. One-step process. To sulfurize the ALD MoOx, the sample was placed in the centre of a tube furnace (1.2 inch in diameter). Initially, the sample was heated at 200 C for 60 min under owing H2 (25 s.c.c.m.) and Ar (25 s.c.c.m.) gas, to remove any organic contaminants on the surface. Subsequently, the temperature was gradually increased from 200 to 1,000 C at 13.3 C min 1, and this temperature was then maintained for 60 min with owing Ar (50 s.c.c.m.)
and H2S (5 s.c.c.m.). Then, the sample was cooled to room temperature under a owing Ar (50 s.c.c.m.) atmosphere.
Two-step process. Initially, samples were annealed at 200 C as in the one-step process. Then, the temperature was gradually increased from 200 C to rstsulfurization temperatures of 600 or 800 C at 13.3 C min 1. The peak temperature (600 or 800 C) was maintained for 60 min with owing Ar(50 s.c.c.m.) and H2S (5 s.c.c.m.). Subsequently, the temperature was gradually increased from the rst-sulfurization temperatures to 1,000 C at 13.3 C min 1 and was maintained at this temperature for 30 min with owing Ar (50 s.c.c.m.)
and H2S (5 s.c.c.m.). The sample was cooled to room temperature under a owing Ar (50 s.c.c.m.) atmosphere after the process was completed. Based on the results shown in Fig. 1, we used a two-step sulfurization process with a 600 C rstsulfurization temperature to sulfurize MoOx and Mo1 xWxOy thin lms in the
MoS2 and Mo1 xWxS2 alloy synthesis process.
Transfer of MoS2 and Mo1 xWxS2. The as-synthesized MoS2 and Mo1 xWxS2
on the SiO2 substrate were coated with polymethyl methacrylate (PMMA) by spin coating at 4,000 r.p.m. for 60 s. After curing of the PMMA at 100 C for 15 min, the samples were immersed in 10% hydrogen uoride solution to etch the SiO2 layer.
Subsequently, the samples were washed using deionized (DI) water and scooped onto a clean SiO2/Si substrate. The PMMA was removed by acetone and washed away using isopropyl alcohol.
Characterization of MoS2 and Mo1 xWxS2. OM (Olympus DX51), Raman
spectroscopy (HORIBA, Lab Ram ARAMIS; 532-nm laser excitation wavelength), AFM (VEECO, Multimode), PL (SPEX1403, SPEX; 532-nm laser excitation wavelength), absorbance with ultravioletvisible spectrophotometer (JASCO Corporation, V-650), XPS (Thermo UK, K-alpha), SEM (JEOL Ltd, JSM-6701F), TEM (FEI Titan G2 Cube 60-300; accelerating voltage, 80 kV), STEM and EDX (JEM 2100F; accelerating voltage, 200 kV) analyses were employed to characterize the MoS2 and Mo1 xWxS2 alloy, and a VCC Mo1 xWxS2 multilayer.
Fabrication and characterization of photodetectors. Photodetectors were fabricated from an as-synthesized VCC Mo1 xWxS2 multilayer, 5l WS2 and 5l
MoS2 on a SiO2 (300 nm)/Si substrate by evaporating Au(40 nm)/Ti(1 nm) electrodes with 100-mm channel length. Electrical measurements were conducted using a Keithley 2400 (Keithley Instruments). The photocurrent was measured by modulating the laser beam with a mechanical chopper (1,000 Hz) and detecting the photocurrent with a current preamplier and a lock-in amplier. A monochromator was used for wavelength-dependent measurements of the photocurrent.
Parameters for analysis of XPS and Raman. We used Spectral Data Processor v4.1 for the XPS and Raman spectra tting. In the tting analysis of the XPS spectra, the full widths at half maximum (FWHM) were between 1.7 and 1.9 eV, the Lorentzian Gaussian Ratio was 2:8, the energy difference between the Mo3d spin-orbit doublet was set to 3.2 eV and the branching ratio was 2/3. In addition, we used Scoeld Relative Sensitivity Factor for calculation of stoichiometry as represented in Supplementary Table 2. For the Raman spectrum tting analysis, the FWHM was between 7 and 12 cm 1.
References
1. Bernardi, M. et al. Extraordinary sunlight absorption and 1 nm-thick photovoltaics using two-dimensional monolayer materials. Nano Lett. 13, 36643670 (2013).
2. Wang, Q. H. et al. Electronics and optoelectronics of two-dimensional transition metal dichalcogenides. Nat. Nanotechnol. 7, 699712 (2012).
3. Chhowalla, M. et al. The chemistry of two-dimensional layered transition metal dichalcogenide nanosheets. Nat. Chem. 5, 263275 (2013).
4. Eda, G. et al. Photoluminescence from chemically exfoliated MoS2. Nano Lett. 11, 51115116 (2011).
5. Mak, K. et al. Atomically thin MoS2: a new direct-gap semiconductor. Phys. Rev. Lett. 105, 136805 (2010).
6. Lee, H. S. et al. MoS2 nanosheet phototransistors with thickness-modulated optical energy gap. Nano Lett. 12, 36953700 (2012).
7. Liu, H. et al. Vapor-phase growth and characterization of Mo1-xWxS2 (0rxr1)
atomic layers on 2-inch sapphire substrates. Nanoscale 6, 624629 (2014).8. Chen, Y. et al. Composition-dependent raman modes of Mo1-xWxS2 monolayer
alloys.. Nanoscale 6, 28332839 (2014).9. Chen, Y. et al. Tunable band gap photoluminescence from atomically thin transition-metal dichalcogenide alloys. ACS Nano 7, 46104616 (2013).
NATURE COMMUNICATIONS | 6:7817 | DOI: 10.1038/ncomms8817 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications 9
& 2015 Macmillan Publishers Limited. All rights reserved.
ARTICLE NATURE COMMUNICATIONS | DOI: 10.1038/ncomms8817
10. Wei, X.-L. et al. Modulating the atomic and electronic structures through alloying and heterostructure of single-layer MoS2. J. Mater. Chem. A 2, 21012109 (2014).
11. Feng, Q. et al. Growth of large-area 2D MoS2(1-x)Se2x semiconductor alloys.
Adv. Mater. 26, 26482653 (2014).12. Xi, J. et al. Tunable electronic properties of two-dimensional transition metal dichalcogenide alloys: a rst-principles prediction. J. Phys. Chem. Lett. 5, 285291 (2013).
13. Lin, Z. et al. Facile synthesis of MoS2 and MoxW1-xS2 triangular monolayers. APL Mater. 2, 092514 (2014).
14. Tannous, J. et al. Synthesis and tribological performance of novelMoxW1 xS2 (0 r x r 1) inorganic fullerenes. Tribol. Lett. 37, 8392 (2010).
15. Yu, Y. et al. Equally efcient interlayer exciton relaxation and improved absorption in epitaxial and non-epitaxial MoS2/WS2 heterostructures. Nano Lett. 15, 486491 (2015).
16. Hong, X. et al. Ultrafast charge transfer in atomically thin MoS2/WS2 heterostructures. Nat. Nanotechnol. 9, 682686 (2014).
17. Komider, K. et al. Electronic properties of the MoS2-WS2 heterojunction. Phys. Rev. B 87, 075451 (2013).
18. Huo, N. et al. Novel and enhanced optoelectronic performances of multilayer MoS2WS2 heterostructure transistors. Adv. Funct. Mater. 24, 70257031 (2014).
19. Jung, Y. et al. Chemically synthesized heterostructures of two-dimensional molybdenum/tungsten-based dichalcogenides with vertically aligned layers. ACS Nano 8, 95509557 (2014).
20. Cheng, R. et al. Electroluminescence and photocurrent generation from atomically sharp WSe2/MoS2 heterojunctionpn diodes. Nano Lett. 14, 55905597 (2014).
21. Tongay, S. et al. Tuning interlayer coupling in large-area heterostructures with CVD-grown MoS2 and WS2 monolayers. Nano Lett. 14, 31853190 (2014).
22. Terrones, H., Lpez-Uras, F. & Terrones, M. Novel hetero-layered materials with tunable direct band gaps by sandwiching different metal disuldes and diselenides. Sci. Rep. 3, 1549 (2013).
23. Gong, Y. et al. Band gap engineering and layer-by-layer mapping of selenium-doped molybdenum disulde. Nano Lett. 14, 442449 (2013).
24. Hyungjun, K. Characteristics and applications of plasma enhanced-atomic layer deposition. Thin Solid Films 519, 66396644 (2011).
25. Kim, H. et al. Applications of atomic layer deposition to nanofabrication and emerging nanodevices. Thin Solid Films 517, 25632580 (2009).
26. Lee, J.-S. et al. Atomic layer deposition of Y2O3 and yttrium-doped HfO2 using a newly synthesized Y(iPrCp)2(N-iPr-amd) precursor for a high permittivity gate dielectric. Appl. Surf. Sci. 297, 1621 (2014).
27. Nam, T. et al. Growth characteristics and properties of Ga-doped ZnO(GZO) thin lms grown by thermal and plasma-enhanced atomic layer deposition. Appl. Surf. Sci. 295, 260265 (2014).
28. Kim, W. H. et al. Signicant enhancement of the dielectric constant through the doping of CeO2 into HfO2 by atomic layer deposition. J. Am. Ceram. Soc. 97, 11641169 (2014).
29. Brahim, C. et al. ZrO2In2O3 thin layers with gradual ionic to electronic composition synthesized by atomic layer deposition for SOFC applications.J. Mater. Chem. 19, 760766 (2009).30. Song, J.-G. et al. Layer-controlled, wafer-scale, and conformal synthesis of tungsten disulde nanosheets using atomic layer deposition. ACS Nano 7, 1133311340 (2013).
31. Blackburn, P. E. et al. The vaporization of molybdenum and tungsten oxides.J. Phys. Chem. 62, 769773 (1958).32. Gutirrez, H. R. et al. Extraordinary room-temperature photoluminescence in triangular WS2 monolayers. Nano Lett. 13, 34473454 (2013).
33. Lin, Y.-C. et al. Wafer-scale MoS2 thin layers prepared by MoO3 sulfurization. Nanoscale 4, 66376641 (2012).
34. Terrones, H. et al. New rst order Raman-active modes in few layered transition metal dichalcogenides. Sci. Rep. 4, 4215 (2014).
35. Li, S.-L. et al. Quantitative raman spectrum and reliable thickness identication for atomic layers on insulating substrates. ACS Nano 6, 73817388 (2012).36. Li, H. et al. From bulk to monolayer MoS2: evolution of Raman scattering. Adv. Funct. Mater. 22, 13851390 (2012).
37. Ling, X. et al. Role of the seeding promoter in MoS2 growth by chemical vapor deposition. Nano Lett. 14, 464472 (2014).
38. Schmidt, H. et al. Transport properties of monolayer MoS2 grown by chemical vapor deposition. Nano Lett. 14, 19091913 (2014).
39. Yu, Y. et al. Controlled scalable synthesis of uniform, high-quality monolayer and few-layer MoS2 lms. Sci. Rep. 3, 1866 (2013).
40. Splendiani, A. et al. Emerging photoluminescence in monolayer MoS2. Nano Lett. 10, 12711275 (2010).
41. Lee, Y. et al. Synthesis of wafer-scale uniform molybdenum disulde lms with control over the layer number using a gas phase sulfur precursor. Nanoscale 6, 28212826 (2014).
42. Van Vechten, J. et al. Electronic structures of semiconductor alloys. Phys. Rev. B 1, 3351 (1970).
43. Yin, W.-J. et al. Origin of the unusually large band-gap bowing and the breakdown of the band-edge distribution rule in the SnxGe1 x alloys. Phys.
Rev. B 78, 161203 (2008).44. Dumcenco, D. O. et al. Visualization and quantication of transition metal atomic mixing in Mo1 xWxS2 single layers. Nat. Commun. 4, 1351 (2013).
45. Garcia, A. et al. Analysis of electron beam damage of exfoliated MoS2 sheets and quantitative HAADF-STEM imaging. Ultramicroscopy 146, 3338 (2014).
46. Elas, A. L. et al. Controlled synthesis and transfer of large-area WS2 sheets: from single layer to few layers. ACS Nano 7, 52355242 (2013).
47. Gong, Y. et al. Vertical and in-plane heterostructures from WS2/MoS2 monolayers. Nat. Mater. 13, 11351142 (2014).
48. Chiu, M.-H. et al. Spectroscopic signatures for interlayer coupling in MoS2-WSe2 van der Waals stacking. ACS Nano 8, 96499656 (2014).
49. Lin, Q. et al. Efcient light absorption with integrated nanopillar/nanowell arrays for three-dimensional thin-lm photovoltaic applications. ACS Nano 7, 27252732 (2013).
50. Aydin, K. et al. Broadband polarization-independent resonant light absorption using ultrathin plasmonic super absorbers. Nat. Commun. 2, 517 (2011).
Acknowledgements
This work was supported by the Center for Integrated Smart Sensors funded by the Ministry of Science, ICT & Future Planning as Global Frontier Project (CISS-2011-0031848), the National Research Foundation of Korea(NRF) grant funded by the Korea government(MSIP) (No. NRF-2014R1A2A1A11052588 and 2011-0013255), and Korea Evaluation Institute of Industrial Technology (KEIT) funded by the Ministry of Trade, Industry and Energy (MOTIE) (Project No. 10050296, Large scale (Over 8) synthesis and evaluation technology of 2D chalcogenides for next generation electronic devices).
Author contributions
J.-G.S. carried out most experiments and analysed the data. G.H.R. and Z.L. contributed to TEM measurement. S.J.L. and J.-M.M. contributed to PL measurement. S.W.S and H.C contributed to photoresponse measurement. C.W.L. contributed to XPS measurement. T.C., H.J. and Y.K. contributed to Raman and AFM measurement. C.D. and C.L.-M. contributed to development and handling of ALD precursor. J.-G.S., J.P. and H.K. designed the experiment and co-wrote the paper. All of the authors discussed the results and commented on the paper.
Additional information
Supplementary Information accompanies this paper at http://www.nature.com/naturecommunications
Web End =http://www.nature.com/ http://www.nature.com/naturecommunications
Web End =naturecommunications
Competing nancial interests: The authors declare no competing nancial interests.
Reprints and permission information is available online at http://npg.nature.com/reprintsandpermissions/
Web End =http://npg.nature.com/ http://npg.nature.com/reprintsandpermissions/
Web End =reprintsandpermissions/
How to cite this article: Song, J. G. et al. Controllable synthesis of molybdenum tungsten disulde alloy for vertically composition-controlled multilayer. Nat. Commun. 6:7817 doi: 10.1038/ncomms8817 (2015).
This work is licensed under a Creative Commons Attribution 4.0 International License. The images or other third party material in this article are included in the articles Creative Commons license, unless indicated otherwise in the credit line; if the material is not included under the Creative Commons license, users will need to obtain permission from the license holder to reproduce the material. To view a copy of this license, visit http://creativecommons.org/licenses/by/4.0/
Web End =http://creativecommons.org/licenses/by/4.0/
10 NATURE COMMUNICATIONS | 6:7817 | DOI: 10.1038/ncomms8817 | http://www.nature.com/naturecommunications
Web End =www.nature.com/naturecommunications
& 2015 Macmillan Publishers Limited. All rights reserved.
You have requested "on-the-fly" machine translation of selected content from our databases. This functionality is provided solely for your convenience and is in no way intended to replace human translation. Show full disclaimer
Neither ProQuest nor its licensors make any representations or warranties with respect to the translations. The translations are automatically generated "AS IS" and "AS AVAILABLE" and are not retained in our systems. PROQUEST AND ITS LICENSORS SPECIFICALLY DISCLAIM ANY AND ALL EXPRESS OR IMPLIED WARRANTIES, INCLUDING WITHOUT LIMITATION, ANY WARRANTIES FOR AVAILABILITY, ACCURACY, TIMELINESS, COMPLETENESS, NON-INFRINGMENT, MERCHANTABILITY OR FITNESS FOR A PARTICULAR PURPOSE. Your use of the translations is subject to all use restrictions contained in your Electronic Products License Agreement and by using the translation functionality you agree to forgo any and all claims against ProQuest or its licensors for your use of the translation functionality and any output derived there from. Hide full disclaimer
Copyright Nature Publishing Group Jul 2015
Abstract
The effective synthesis of two-dimensional transition metal dichalcogenides alloy is essential for successful application in electronic and optical devices based on a tunable band gap. Here we show a synthesis process for Mo1-x Wx S2 alloy using sulfurization of super-cycle atomic layer deposition Mo1-x Wx Oy . Various spectroscopic and microscopic results indicate that the synthesized Mo1-x Wx S2 alloys have complete mixing of Mo and W atoms and tunable band gap by systematically controlled composition and layer number. Based on this, we synthesize a vertically composition-controlled (VCC) Mo1-x Wx S2 multilayer using five continuous super-cycles with different cycle ratios for each super-cycle. Angle-resolved X-ray photoemission spectroscopy, Raman and ultraviolet-visible spectrophotometer results reveal that a VCC Mo1-x Wx S2 multilayer has different vertical composition and broadband light absorption with strong interlayer coupling within a VCC Mo1-x Wx S2 multilayer. Further, we demonstrate that a VCC Mo1-x Wx S2 multilayer photodetector generates three to four times greater photocurrent than MoS2 - and WS2 -based devices, owing to the broadband light absorption.
You have requested "on-the-fly" machine translation of selected content from our databases. This functionality is provided solely for your convenience and is in no way intended to replace human translation. Show full disclaimer
Neither ProQuest nor its licensors make any representations or warranties with respect to the translations. The translations are automatically generated "AS IS" and "AS AVAILABLE" and are not retained in our systems. PROQUEST AND ITS LICENSORS SPECIFICALLY DISCLAIM ANY AND ALL EXPRESS OR IMPLIED WARRANTIES, INCLUDING WITHOUT LIMITATION, ANY WARRANTIES FOR AVAILABILITY, ACCURACY, TIMELINESS, COMPLETENESS, NON-INFRINGMENT, MERCHANTABILITY OR FITNESS FOR A PARTICULAR PURPOSE. Your use of the translations is subject to all use restrictions contained in your Electronic Products License Agreement and by using the translation functionality you agree to forgo any and all claims against ProQuest or its licensors for your use of the translation functionality and any output derived there from. Hide full disclaimer