INTRODUCTION
With the rapid development of the smart grid, advanced electric field measurement technology is increasingly required, which is one of the most significant segments to ensure the normal operation of power equipment [1, 2]. The amplitude and frequency composition of an electric field becomes more complex accompanied by the introduction of a large number of power electronic devices [3]. Traditional sensors are prone to resonance and need a carrier light source [4, 5], while the sensors based on the electroluminescence effect have the advantages of excellent electrical insulation performance and distributed measurement [6–8]. Electroluminescence refers to a solid luminescence phenomenon, in which composites convert the electric energy into optical energy [9, 10]. Electrons will be accelerated under the action of the electric field, causing the occurrence of collision excitation and ionization [11, 12], and photons are emitted when the electrons transition from the excited state back to the ground state [13–15].
Due to the advantages of uniform luminescence and high efficiency [16–18], research on the preparation of electroluminescence devices has received extensive attention. Jun S [19] et al. used ZnS:Cu/PVB as a luminescent layer and prepared stretchable electroluminescent devices with excellent mechanical properties. However, considering the high voltage required to achieve high electroluminescence intensity, the practical engineering application of electroluminescent devices is limited, and problems such as energy waste will arise [20–22]. Improving the electroluminescence intensity of luminescent layer composites is the key to enhance the performance of electroluminescent devices [23–25]. Jun S Y [26] et al. introduced short carbon nanotubes treated with chlorobenzene to improve the luminance of devices. Gupta [27] et al. introduced rGO particles and found that the luminance of devices with 0.5 wt% rGO particles was the strongest.
It can be visualised that the electroluminescence characteristics of ZnS:Cu particles are related to the quantum process of electron transition [28]. Therefore, it is necessary to study the electroluminescence properties of ZnS:Cu particles from the microscopic point of view, which is inadequate in this area [29]. Density functional theory (DFT), as a powerful tool, is widely used to calculate the band structure of ZnS:Cu particles [30, 31]. Traditional DFT methods including local density approximation and generalised gradient approximation (GGA) cannot describe the electronic properties precisely, leading to the serious underestimation of ZnS:Cu bandgap [32]. By introducing a specific Hubbard parameter U, DFT + U method can accurately correct the delocalisation of d electrons (especially d electrons in transition metals) [33], which has attracted extensive attention. Sharma M et al. [34] calculated the band structure of ZnS particles based on the DFT + U method, and the calculated results are consistent with the theory.
Despite the achievements having been made so far, few studies concern about the relationship between the electroluminescence mechanism and filler intrinsic attributes, and the research on how to improve the electroluminescence intensity of composites is also insufficient. In this paper, we adopt a simple solution-processing method to prepare ZnS:Cu/epoxy composites, which is majorly applied to the luminescent layer of the devices. The effects of electric field strength, filler mass fraction and frequency on the electroluminescence intensity of composites have been studied. High temperature-sintered barium titanate (BaTiO3) and Zinc oxide whisker (ZnOw) particles have been introduced to improve the dielectric constant of the matrix [35–37], and consequently improve the electroluminescence intensity of composites. The finite element method is used to prove the positive effect of the increased dielectric constant of matrix on the enhanced electroluminescence intensity. The density functional theory + U method is adopted to analyse the electroluminescence characteristics of ZnS:Cu/epoxy composites from the microscopic point of view. The specific research framework is shown in Figure 1.
[IMAGE OMITTED. SEE PDF]
MATERIALS AND METHODS
Materials and sample preparation
The raw materials used in the experiments are listed in Supporting Information. Composites with different filler mass fractions and different introduced ceramic fillers are prepared for the subsequent electroluminescence tests. The experimental flow chart is shown in Figure 2a.
-
The required epoxy resin is poured into a beaker with the curing agent added in a ratio of 100:85. The flask is heated in a vacuum oven at 60°C, so that the viscosity of epoxy resin can be slightly reduced and the fluidity of the matrix can be increased.
-
The fillers are weighed according to the required proportion and added to the epoxy resin mixture. The mixture is poured into a three-necked flask and placed in an oil bath with the temperature controlled at 60°C and the speed of 300 r/min. The mixture is stirred for 1 h. When the matrix and fillers are fully mixed, accelerant is added in a ratio of 100:1 and stirred for 10 min.
-
The mixed solution is poured into a dry beaker and put into a vacuum drying oven at 60°C for several vacuumising operations until there are no bubbles on the surface.
-
The mould sprayed with the release agent is put into the blast dryer to preheat, and the blast dryer is preheated at 100°C for 10 min. Then the vacuumised mixed solution is poured into the mould and dried in the oven again. The oven temperature is set to 100°C for 4 h and then raised to 150°C for 10 h to prepare the required composites.
[IMAGE OMITTED. SEE PDF]
Experimental platform
The schematic and practical diagrams of the experimental platform are shown in Figure 2b–c. High voltage AC power, voltage probe and oscilloscope are used for electroluminescence tests. Spectral luminance metre is used to test the electroluminescence intensity of composites.
Microstructure and luminescence analysis
Scanning electron microscopy is used to observe the morphology of ZnS:Cu, BaTiO3 and ZnOw particles, and the overall distribution of particles in ZnS:Cu/epoxy, ZnS:Cu/BaTiO3/epoxy and ZnS:Cu/ZnOw/epoxy composites. As shown in Figure 3a–c, ZnS:Cu particles are irregularly granular and the particle size is on the order of micron grade. BaTiO3 particles clump together and the particle size is much smaller than that of ZnS:Cu particles. ZnOw particles have distinct acicular structure. It can be seen from Figure 3d–f that the filler particles evenly distribute in the matrix, the interface bonding strength between particles and the matrix is excellent, and no obvious defects and voids are observed. The three small figures embedded in the upper right corners are ZnS, BaTiO3 and ZnOw particles, respectively. BaTiO3 with small particle size and ZnOw with needle shape help to fill the gaps between ZnS:Cu particles, thus forming a denser luminescent layer.
[IMAGE OMITTED. SEE PDF]
The samples are all wafers with a diameter of 70 mm and thickness of 1.5 mm. In the dark situation, the voltage is applied after the luminance of samples is completely attenuated. After a period of pressurisation, it is found that the luminescence phenomenon first occurs near the electrode, and it is a distinct green light as shown in Figure 3g. The Commission Internationale de L'Eclairage (CIE) coordinate (X, Y) is used to quantitatively represent the luminescent colours [38, 39], where X represents the red component and Y represents the green component. As shown in Figure 3h, all the monochromatic light lies on the tongue curve, and the specific location of the colour light emitted by the sample is marked as (0.2413, 0.5915), which is within the range of green light. A fluorescence spectrophotometer is used for spectral tests as shown in Figure 3i. It is found that when excited by 375 nm light, the strongest emission peak of ZnS:Cu is located at 533 nm, which is in the range of green light band. A UV-Vis absorption spectrometer is used to test the UV-Vis diffuse reflection spectrum of ZnS:Cu particles. The data interval is set to 1.0 nm and the scan speed is set to medium speed.
Electric breakdown testing
In the room temperature, the breakdown strength tester HCDJC-50 kV is used for the electric breakdown test. We apply pressure at 2 kV/s until the sample is punctured. Ten samples are tested in each group for subsequent analysis.
RESULT AND DISCUSSION
Relationship between electroluminescence intensity and electric field strength and filler mass fraction
ZnS:Cu/epoxy composites with filler mass fraction of 55 wt%, 60 wt%, 65 wt%, 70 wt% and 75 wt% are prepared to study the relationship between electroluminescence intensity and electric field strength. Considering that the sample emits obvious green light under the action of the electric field. The proportion of green in the three primary colours (G) is taken as the characteristic value to represent the electroluminescence intensity of composites in this paper, which is specified as equation (1).
In order to ensure the safety of experiments, the breakdown electric field strength of composites under the AC electric field is tested first. Weibull distribution [40, 41] is used to process the breakdown electric field strength data and shown in equation (2).
The least square method and Ross failure probability distribution function are used to solve the correlation coefficient, and the correlation formula is as follows.
The Ross failure probability distribution function is shown in equation (3).
The breakdown electric field strength data are arranged in an increasing order and the correlation coefficients are calculated by the least square method of linear fitting as shown in equation (4).
The experimental data processing results are shown in Figure 4a.
[IMAGE OMITTED. SEE PDF]
It is found that the breakdown electric field strength of composites is all above 10 kV/mm. With the increase of filler mass fraction, the breakdown electric field strength of composites first increases and then decreases. When the mass fraction of ZnS:Cu particles reaches 65 wt%, the breakdown electric field strength of composites has a maximum value of 21.91 kV/mm. The minimum excitation electric field strength required for luminescence is also tested, and it is found that the initial excitation electric field strength of composites is no greater than 2 kV/mm. The comparison of the minimum excitation electric field strength required for luminescence and breakdown electric field strength is shown in Figure 4b. The breakdown electric field strength is much stronger than the minimum excitation electric field strength, which not only ensures safety, but also has practical application value. Thus, in the subsequent experiments, the pressurisation time is controlled for 10 min, and the electroluminescence intensity of composites with different filler mass fractions is tested under the electric field strength of 2, 3, 4, 5 and 6 kV/mm, respectively.
Figure 4c shows the relationship between electroluminescence intensity and filler mass fraction under different electric field strength at 50 Hz. It can be seen that with the increase of filler mass fraction, the electroluminescence intensity of composites shows an overall upward trend, and when the electric field strength reaches 3 kV/mm, the upward trend is more obvious. Especially, when the electric field strength goes up to 4 kV/mm, the electroluminescence intensity of composites with 75 wt% filler mass fraction is 147.4% than that of composites with 55 wt% filler mass fraction. This can be explained that with the increase of the filler mass fraction, the number of luminescence centres increases, and more electrons collide with the luminescent centres, thus enhancing the electroluminescence intensity of composites. The saturation is achieved when the filler concentration reaches 75 wt%, and the composite could not be poured with further addition of ZnS:Cu particles. The relationship between electroluminescence intensity and electric field strength with different filler mass fraction at 50 Hz is shown in Figure 4d. With the increase of electric field strength, the electroluminescence intensity of composites increases gradually. This is due to that with the increase of electric field strength, on the one hand, the electrons attain more energy, which is favourable for the occurrence of electron collision and ionization, thus doubling the number of electrons. On the other hand, more electrons collide with the luminescence centre, which is in favour of the excitation and de-excitation of electrons to produce photons, and ultimately improves the electroluminescence intensity. When the mass fraction of the filler is low, the electroluminescence intensity of composites increases more with the increase of electric field strength, especially for the composites with a filler mass fraction of 55 wt%. When the electric field strength increases from 2 kV/mm to 6 kV/mm, the electroluminescence intensity of composites with 55 wt% filler mass fraction increases by 125.1%, and the electroluminescence intensity of composites with filler mass fraction of 60 wt% and 65 wt% increases almost linearly with the increase of electric field strength.
Figure 4e shows the luminescence photographs of composites with different filler mass fractions (55 wt%, 60 wt%, 65 wt%, 70 wt% and 75 wt%) under the electric field strength of 5 kV/mm. Due to the randomness of electron migration path and filler distribution [42], the luminescence region is not always symmetrical. It can be found that with the increase of the filler mass fraction, the luminous range of composites becomes larger due to the increase of the probability of electron collision with luminescence centre at each position [43]. Figure 4f shows the luminescence photographs of 65 wt% ZnS:Cu/epoxy composites under different electric field strength (2, 3, 4, 5 and 6 kV/mm). When the applied electric field strength is 2 kV/mm, the luminance of composite is very low and only the circle near the electrode emits light. With the increase of applied electric field strength, the luminous range becomes larger and the emitted green light is more obvious.
In order to further study the relationship between electroluminescence characteristics and electronic structure of ZnS:Cu particles, DFT calculation is carried out based on the plane wave pseudopotential method to optimise the geometric configuration of ZnS:Cu particles [44, 45], and the band structure of ZnS:Cu particles under different electric field strength is compared.
In cubic ZnS, the Zn atom is located at (0, 0, 0) and S atom is located at (0.25, 0.25, 0.25), which has a face-centred cubic crystal structure [46]. Each Zn atom is surrounded by four S atoms, and each S atom is surrounded by four Zn atoms, which can exist stably in nature. Firstly, a 2 × 2 × 1 supercell is established on the basis of the ZnS protocell. The ZnS supercell contains 32 atoms (16 Zn atoms and 16 S atoms). When considering doping, the most likely doping model in ZnS is the substitution doping of the Cu atom instead of the Zn atom, both Cu atom and Zn atom vacancy at the gap position cannot exist stably [47, 48]. Therefore, the following calculation only considers the form of substitution doping in which a Cu atom replaces a Zn atom. The model is shown as Figure 5a.
[IMAGE OMITTED. SEE PDF]
Geometric optimization should be carried out before calculation. The commutative correlation function is approximated by GGA's (Generalised gradient approximations) PBE (Perdew–Burke–Ernzerhof) functional, and the GGA + U method is applied to introduce a specific Hubbard potential to correct the problem of bandgap underestimation in the GGA method [34, 45]. The supersoft pseudopotential is used to describe the interaction between valence electrons and the real ion.
The band structure of ZnS:Cu particles without the electric field is calculated first as shown in Figure 5b. In practical studies, we are more concerned with the band distribution near the Fermi level, so the figures only show the electron energy distribution in the valence band and conduction band near the Fermi level. The calculated bandgap of ZnS:Cu particles is 2.831 eV; the lowest point of conduction band and the highest point of valence band are both at the same K-point (G), indicating the direct bandgap semiconductor material of ZnS:Cu. In order to further study the electronic structure of ZnS:Cu particles, density of states (DOS) of Zn, S and Cu atoms are calculated as shown in Figure 5c. It can be seen that the conduction band of 3–6 eV mainly comes from the contribution of Zn 4s and 3p states, and the upper valence band region located in the energy range of −6–0 eV mainly relates to the contribution of S 3p and Cu 3d states. The hybridisation of S 3p and Cu 3d broadens the valence band of ZnS:Cu and forms a p-d hybridisation peak, which corresponds to a shallow acceptor level. Electrons in the valence band can first jump to this impurity level, and then to the conduction band, which is beneficial to the absorption of visible light of ZnS. UV-Vis the diffuse reflection spectrum of ZnS:Cu particles which is tested to compare with the calculated value as shown in Figure 5d. The bandgap is determined by Tauc plot from the analysis of the absorption spectrum in Figure 5e [49] as shown in equation (5).
The bandgap of ZnS:Cu particles under different electric field strength is shown in Table 1.
TABLE 1 The calculated bandgap of ZnS:Cu particles under different electric field strengths
Electric field strength (kV/mm) | 0 | 5 | 10 | 50 | 100 |
Bandgap of ZnS:Cu particle (eV) | 2.831 | 2.829 | 2.816 | 2.764 | 2.682 |
ZnS:Cu particle has a narrower bandgap when an electric field is applied, which may be due to that the energy band has a tendency to expand and moves slightly in the direction of the Fermi level with the increase of electric field strength, leading to the decrease of bandgap, and when the electric field strength exceeds 10 kV/mm, this phenomenon is more obvious. The reduction of bandgap is beneficial to the transfer of electrons from occupied orbit to vacant orbit and the emission of photons, which contributes to the enhancement of composite electroluminescence intensity.
Research on improving the electroluminescence intensity of composites
The low luminance of composites impedes the practical implementation. To enhance the performance of ZnS:Cu/epoxy composites and expand the scope of practical engineering application, studies on how to improve the electroluminescence intensity of composites have been carried out. The dielectric constant of the matrix can be improved by introducing ceramic fillers, so that the electric field can be concentrated near the phosphor particles [8]. This contributes to the occurrence of collision excitation and ionization of electrons [50], and also the reduction of interface refractive index difference between the matrix and the phosphor particles, which makes it easier for the light to pass through the matrix, and consequently enhances the electroluminescence intensity.
The BaTiO3 particle sintered at high temperature has the advantages of high dielectric constant and low price, which is widely used in the electric field [51, 52]. The ZnOw particle is a wide bandgap semiconductor with high exciton binding energy, which has great application potential in the field of optoelectronics [53]. According to the results in the previous sections, when the filler mass fraction is low, the electroluminescence intensity of composites cannot meet expectations, while as the mass fraction of fillers increases to 75 wt%, the agglomeration risk will increase, which damages the electrical and mechanical properties of composites. The filler mass fraction of 65 wt% reaches the optimal trade-off. The breakdown electric field strength is higher than that in other cases, and the electroluminescence intensity is also relatively high. Therefore, the mass fraction of ZnS:Cu fillers is controlled at 65 wt%, 1 wt% and 5 wt% BaTiO3 and ZnOw particles are introduced, respectively, to study the effects of the introduction of ceramic fillers on the electroluminescence intensity of composites.
The breakdown electric field strength of composites is tested first, and the results are shown in Figure 6a. With the increase of the mass fraction of ceramic fillers, the breakdown electric field strength decreases gradually. Compared with BaTiO3 introduced composites, the breakdown electric field strength decreases more obviously after the introduction of ZnOw particles, which may be related to the irregular shape of ZnOw particles [54]. Especially after the introduction of 5 wt% ZnOw particles, the breakdown electric field strength reduces to 7.72 kV/mm, which is 35.25% of the pure ZnS:Cu/epoxy composites. The low breakdown electric field strength of composites is not conducive to the subsequent research and practical applications. Therefore, only 1 wt% BaTiO3, 5 wt% BaTiO3 and 1 wt% ZnOw particles are selected to study the effects of their introduction on the electroluminescence intensity of composites, expressed as ZnS:Cu-BaTiO3-1, ZnS:Cu-BaTiO3-5 and ZnS:Cu-ZnOw-1, respectively.
[IMAGE OMITTED. SEE PDF]
The results are shown in Figure 6b. Compared with pure ZnS:Cu/epoxy composites, the electroluminescence intensity of composites can be improved by introducing BaTiO3 and ZnOw particles. The particle size of ZnS:Cu particles is about 20 times than that of BaTiO3 particles. Therefore, BaTiO3 particles can fill the gap between ZnS:Cu particles and form a denser luminescent layer. When the mass fraction of introduced BaTiO3 particles is 1 wt%, the electroluminescence intensity of composites increases most obviously. The electroluminescence intensity of composites with 5 wt% BaTiO3 particles is lower than that with 1 wt% BaTiO3 particles, which may be due to that the high concentration of fillers result in the occurrence of agglomeration, and it is not conducive to the collision and excitation of electrons [6, 55]. Moreover, an increase in filling concentration may lead to an increase in defects and leakage current, which produces the blocking effects in the luminescence of composites.
For the purpose of further investigating the fundamental electroluminescence mechanism of ZnS:Cu based composites and the effects of the introduction of ceramic fillers on the luminance of composites, a two-dimensional model is established based on the SEM diagram, and the finite element method is used to calculate the potential and electric field distribution as shown in Figure 7a–b and Figure S1. The relative dielectric constant of the ZnS:Cu particles is set as 9.6 [37], and that of matrix as 3 [56]. The results are shown in Figure 7c–f.
[IMAGE OMITTED. SEE PDF]
On account of the irregular shape of ZnS particles, there is a large amount of charge accumulation at the tip, so the electric field strength here is the largest, and the electric field strength inside the matrix is greater than that inside the ZnS particles. Figure 7d–f represent the electric field distribution of the matrix and the ZnS:Cu particles when the dielectric constant of the matrix equals to 3, 5 and 8, respectively. It can be found that with the increase of the dielectric constant of matrix, the electric field strength inside ZnS:Cu particles increases gradually (from dark blue to light blue), indicating that when the dielectric constant of matrix is higher, the electric field strength inside ZnS:Cu particles is higher, which is more conducive to the excitation and ionization of electrons and the improvement of electroluminescence intensity.
The average value of phosphor particle surface electric field strength is denoted as , and the average value of matrix surface electric field strength is denoted as . The simulation results are shown as Figure 7g. As the dielectric constant of the matrix increases, the electric field strength of the matrix decreases and that of the phosphor particles increases, the gap of electric field strength between the matrix and the phosphor particles becomes smaller and smaller. This also helps to solve the problem of excessively large local electric field strength, so as to improve the breakdown field strength. Moreover, the larger the is, the more favourable it is for the electrons to collide with the luminescence centre and improve the luminescence intensity. The measured frequency-dependent dielectric constants for the four kinds of composites are shown in Figure 7h. The dielectric constant of composites increases obviously after adding ceramic fillers. The results verify that the highly polarized matrix by introducing ceramic fillers can concentrate the electric field on phosphor particles and boost the electroluminescence intensity of composites.
Relationship between electroluminescence intensity and voltage frequency
We select four kinds of composites to study the relationship between electroluminescence intensity and voltage frequency, which is 65 wt% ZnS:Cu, 65 wt% ZnS:Cu-BaTiO3-1, 65 wt% ZnS:Cu-BaTiO3-5 and 65 wt% ZnS:Cu-ZnOw-1 composite, respectively. Electroluminescence intensity of these composites are studied under 3 kV/mm and 5 kV/mm as the frequency changes from 50 to 450 Hz. The specific results are shown as Figure 8.
[IMAGE OMITTED. SEE PDF]
Figure 8a shows the relationship between electroluminescence intensity and frequency under the electric field strength of 3 kV/mm. It is found that with the increase of frequency, the electroluminescence intensity of composites increases gradually, and the electroluminescence intensity of composites with the introduction of ceramic fillers is always greater than that of the pure ZnS:Cu/epoxy composites. It has the sharpest increase when the frequency increases from 150 to 250 Hz; this is because when the voltage frequency increases, the number of electron accelerations per unit time increases, resulting in an increase in the number of collisions, and eventually improves the electroluminescence intensity. When the frequency increases from 350 to 450 Hz, the amplitude of electroluminescence intensity enhancement is relatively small. This may be due to that electron energy plays a dominant role this time, the increase of frequency will shorten the acceleration time of electrons, and reduce the corresponding electron energy as shown in Figure 9. The electrons cannot jump to the conduction band to release photons with insufficient energy.
[IMAGE OMITTED. SEE PDF]
Figure 8b shows the relationship between electroluminescence intensity of composites and voltage frequency under the electric field strength of 5 kV/mm. The variation law is consistent with the trend of composites under 3 kV/mm. The luminescence photographs of 65 wt% ZnS:Cu-BaTiO3-1 composites at the frequency of 50 Hz, 150 Hz, 250 Hz, 350 and 450 Hz under the electric field strength of 3 kV/mm and 5 kV/mm are shown as Figure 8c–d. It is found that with the increase of frequency, the luminescence range expands and the luminescence phenomenon is more obvious, which is consistent with the above analysis.
CONCLUSION
In summary, we demonstrate a transparent light-emitting composite with electroluminescence property. The effects of electric field strength, filler mass fraction, voltage frequency and the introduction of ceramic fillers on the electroluminescence intensity of composites have been studied. the finite element method is used to discuss the effect of the dielectric constant of the matrix on the electric field distribution in the matrix and fillers, and then the electroluminescence intensity of composites. The density functional theory + U method is applied to analyse the intrinsic relationship between electroluminescence intensity and the microscopic structure of ZnS:Cu. This study provides the basis for optimising the electroluminescence characteristics by understanding the relationship between electroluminescence principle and filler attributes, and analyses the potential application of electroluminescent composites in the electric field measurement field as shown in Supporting information. The specific conclusions are as follows:
-
When the applied electric field strength is constant, the electroluminescence intensity of composites increases gradually with the increase of the filler mass fraction. This can be explained that with the increase of the filler mass fraction, more luminescent centres are introduced, which is favourable for electron transition to produce photons. When the filler mass fraction is constant, the electroluminescence intensity of composites continuously rises with the enhancement of applied electric field strength. This is due to the higher energy of electrons and the narrower bandgap of ZnS:Cu particles, which are conducive to the electron collision excitation and ionization. As a result, the electroluminescence intensity of composites is enhanced.
-
The introduction of BaTiO3 and ZnOw particles is beneficial to the enhancement of electroluminescence intensity of composites. It is studied from two aspects, experiment and simulation that the dielectric constant of the matrix can be enhanced with the introduction of BaTiO3 and ZnOw particles, leading to the concentration of the electric field near the phosphor particles, which contributes to the excitation and ionization of electrons, thus enhancing the electroluminescence intensity of composites. This positive effect is related to both the type and concentration of the introduced fillers, and it is most obvious with the introduction of 1 wt% BaTiO3 particles.
-
The electroluminescence intensity of composites gradually increases with the increase of voltage frequency, and the luminous range has a trend of diffusion according to the photographs. The reasons are as follows: when the frequency of applied voltage rises, the number of electron accelerations per unit time adds, resulting in an increase in the number of electron collisions to excite the luminescence centre, thus improving the electroluminescence intensity. As the frequency constantly increases, the amplitude of electroluminescence intensity enhancement tends to decrease, which may be attributed to the inadequate acceleration time of electrons and the corresponding insufficient energy, which blocks the generation of photons.
ACKNOWLEDGEMENTS
This work was supported by National Natural Science Foundation of China (No.51877082), and Science and Technology Project of State Grid Corporation of China (No.7000-202158440A-0-0-00).
CONFLICT OF INTEREST
The author declares that there is no conflict of interest that could be perceived as prejudicing the impartiality of the research reported.
DATA AVAILABILITY STATEMENT
Data that support the findings of this study are available from the corresponding author upon reasonable request.
Ma, G., et al.: Optical sensors for power transformer monitoring: a review. High Volt. 6(3), 367–386 (2021)
Wang, Y., et al.: Simulations and experiments of the generation apparatus of the DC electric field with the space charge. High Volt. 6(6), 1061–1068 (2021)
Han, Z., et al.: Micro‐cantilever capacitive sensor for high‐resolution measurement of electric fields. IEEE Sensors J. 21(4), 4317–4324 (2020)
Zheng, J., et al.: Equipotential shielding voltage sensor for contact measurement of transient voltage in EHV/UHV power grids. High Volt. 6(2), 291–301 (2021)
Cui, Y., Zhuang, C., Zeng, R.: Electric field measurements under DC corona discharges in ambient air by electric field induced second harmonic generation. Appl. Phys. Lett. 115(24), [eLocator: 244101] (2019)
Jayathilaka, W., et al.: Alternative current electroluminescence and flexible light emitting devices. J. Mater. Chem. C 7(19), 5553–5572 (2019)
Zhang, X., Wang, F.: Recent advances in flexible alternating current electroluminescent devices. Apl. Mater. 9(3), [eLocator: 030701] (2021)
Qu, C., et al.: Multifunctional displays and sensing platforms for the future: a review on flexible alternating current electroluminescence devices. ACS Appl. Electron. Mater. 3(12), 5188–5210 (2021)
Brubaker, C.D., et al.: 3D‐Printed alternating current electroluminescent devices. J. Mater. Chem. C 7(19), 5573–5578 (2019)
Wei, X.Y., et al.: Fully‐integrated motion‐driven electroluminescence enabled by triboelectrification for customized flexible display. Nano Energy 61, 158–164 (2019)
Fang, H., et al.: Self‐powered flat panel displays enabled by motion‐driven alternating current electroluminescence. Nano Energy 20, 48–56 (2016)
Gahlmann, T., et al.: Bifacial color‐tunable electroluminescent devices. ACS Appl. Mater. Interfaces 13(24), 28514–28520 (2021)
Liang, G., et al.: Coaxial‐structured weavable and wearable electroluminescent fibers. Adv. Electron. Mater. 3(12), [eLocator: 1700401] (2017)
Sun, J., et al.: MXene enhanced self‐powered alternating current electroluminescence devices for patterned flexible displays. Nano Energy 86, [eLocator: 106077] (2021)
Janczak, D., et al.: Stretchable and washable electroluminescent display screen‐printed on textile. Nanomaterials 9(9), [eLocator: 1276] (2019)
Wang, J., et al.: Highly stretchable and self‐deformable alternating current electroluminescent devices. Adv. Mater. 27(18), 2876–2882 (2015)
Xie, P., Mao, J., Luo, Y.: Highly bright and stable electroluminescent devices with extraordinary stretchability and ultraconformability. J. Mater. Chem. C 7(3), 484–489 (2019)
Liang, G., et al.: Highly flexible and bright electroluminescent devices based on Ag nanowire electrodes and top‐emission structure. Adv. Electron. Mater. 3(3), [eLocator: 1600535] (2017)
Jun, S., et al.: Extremely flexible, transparent, and strain‐sensitive electroluminescent device based on ZnS:Cu‐polyvinyl butyral composite and silver nanowires. Appl. Surf. Sci. 429, 144–150 (2018)
Shanker, R., et al.: Solution‐processable, high‐performance flexible electroluminescent devices based on high‐k nanodielectrics. Adv. Funct. Mater. 29(39), [eLocator: 1904377] (2019)
Shin, H., et al.: Stretchable electroluminescent display enabled by graphene‐based hybrid electrode. ACS Appl. Mater. Interfaces 11(15), 14222–14228 (2019)
Zhou, Y., et al.: Stretchable high‐permittivity nanocomposites for epidermal alternating‐current electroluminescent displays. ACS Materials Lett. 1(5), 511–518 (2019)
Singh, P., et al.: Optimization of processing parameters for designing an efficient AC driven powder electroluminescent device. Ceram. Int. 42(15), 17016–17022 (2016)
Jiang, Y., et al.: Enhanced dielectric performance of P(VDF‐HFP) composites with satellite–core‐structured Fe2O3@BaTiO3 nanofillers 11(10), [eLocator: 1541] (2019)
Stauffer, F., Tybrandt, K.: Bright stretchable alternating current electroluminescent displays based on high permittivity composites. Adv. Mater. 28(33), 7200–7203 (2016)
Jun, S.Y., et al.: Chlorobenzene‐treated carbon nanotubes in a dielectric layer and their impact on inorganic electroluminescence. Carbon 146, 462–467 (2019)
Gupta, B.K., et al.: A novel electroluminescent device based on a reduced graphene oxide wrapped phosphor (ZnS:Cu, Al) and hexagonal‐boron nitride for high‐performance luminescence. Nanoscale 9(15), 5002–5008 (2017)
Blades, C.D.J., Walker, A.B.: Simulation of organic light‐emitting diodes. Synth. Met. 111, 335–340 (2000)
Wang, V., Zhao, Y., Javey, A.: Performance limits of an alternating current electroluminescent device. Adv. Mater. 33(2), [eLocator: 2005635] (2021)
Gui, Y., et al.: Platinum modified MoS2 monolayer for adsorption and gas sensing of SF6 decomposition products: a DFT study. High Volt. 5(4), 454–462 (2020)
Shaili, H., et al.: Structural, electronic and optical properties of Cu‐doped ZnS thin films deposited by the ultrasonic spray method‐DFT study. Opt. Quant. Electron. 53(6), 1–14 (2021)
Liu, M., et al.: Understanding of electronic and optical properties of ZnS with high concentration of point defects induced by hot pressing process: the first‐principles calculations. Comput. Mater. Sci. 174, [eLocator: 109492] (2020)
Hedjar, H., et al.: First‐principles studies of electronic structure, magnetic and optical properties of rare‐earth (RE= Sm, Eu, Gd, and Er) doped ZnS. Comput. Condens. Matter 30, [eLocator: e00632] (2022)
Sharma, M., Mishra, D., Kumar, J.: First‐principles study of the structural and electronic properties of bulk ZnS and small ZnnSn nanoclusters in the framework of the DFT+U method. Phys. Rev. B 100(4), [eLocator: 045151] (2019)
Hu, J., et al.: Improved dielectric properties of polypropylene‐based nanocomposites via co‐filling with zinc oxide and barium titanate. Compos. Sci. Technol. 148, 20–26 (2017)
Ma, L., Zhang, J., Teng, C.: Covalent functionalization of aramid fibers with zinc oxide nano‐interphase for improved UV resistance and interfacial strength in composites. Compos. Sci. Technol. 188, [eLocator: 107996] (2020)
Wang, X., et al.: Stretchable and transparent electroluminescent device driven by triboelectric nanogenerator. Nano Energy 58, 410–418 (2019)
Konovalenko, I.A., et al.: ProLab: a perceptually uniform projective color coordinate system. IEEE Access 9, 133023–133042 (2021)
Tang, H., et al.: A novel polymethyl methacrylate derivative grafted with cationic iridium (III) complex units: synthesis and application in white light‐emitting diodes. Polymers 11(3), [eLocator: 499] (2019)
Zhang, Z., et al.: Influence of morphological variations on the AC breakdown of XLPE insulation in submarine cable factory joints. High Volt. 5(1), 69–75 (2020)
Khaled, U., Beroual, A., Khan, Y.: Statistical investigation of AC breakdown voltage of natural ester with electronic scavenger additives. IEEE Trans. Dielectr. Electr. Insul. 26(6), 2012–2018 (2019)
Ganose, A.M., et al.: Efficient calculation of carrier scattering rates from first principles. Nat. Commun. 12(1), 1–9 (2021)
Giannini, S., et al.: Quantum localization and delocalization of charge carriers in organic semiconducting crystals. Nat. Commun. 10(1), 1–12 (2019)
Li, Y., et al.: DFT simulation on interaction of H2O molecules with ZnS and Cu‐activated surfaces. J. Phys. Chem. C 123(5), 3048–3057 (2019)
Pham, H.H., Barkema, G.T., Wang, L.W.: DFT+ U studies of Cu doping and p‐type compensation in crystalline and amorphous ZnS. Phys. Chem. Chem. Phys. 17(39), 26270–26276 (2015)
Nouri, R., et al.: Investigation of opto‐electronic properties of ZnS polymorphs through modified Becke‐Johnson exchange potential. Optik 130, 1004–1013 (2017)
Warkentin, M., et al.: Electroluminescence materials ZnS: Cu, Cl and ZnS:Cu, Mn, Cl studied by EXAFS spectroscopy. Phys. Rev. B 75(7), [eLocator: 075301] (2007)
Car, B., et al.: Probing the local structure of dilute Cu dopants in fluorescent ZnS nanocrystals using EXAFS. Nanoscale 3(10), 4182–4189 (2011)
Jubu, P.R., et al.: Tauc‐plot scale and extrapolation effect on bandgap estimation from UV–vis–NIR data–A case study of β‐Ga2O3. J. Solid State Chem. 290, [eLocator: 121576] (2020)
Wang, L., et al.: Advances in alternating current electroluminescent devices. Adv. Opt. Mater. 7(7), [eLocator: 1801154] (2019)
Cao, M., et al.: Greatly enhanced permittivity in BaTiO3‐epoxy dielectric composites with improved connectivity of ceramic phase. J. Materiomics 7(1), 1–7 (2021)
Wu, W., et al.: Inserting insulating barriers into conductive particle channels: A new paradigm for fabricating polymer composites with high dielectric permittivity and low dielectric loss. Compos. Sci. Technol. 216, [eLocator: 109070] (2021)
Li, W., et al.: Enhancing light emission in flexible AC electroluminescent devices by tetrapod‐like zinc oxide whiskers. Opt Express 24(20), [eLocator: 23419] (2016)
Lu, Y., et al.: Bio‐inspired polydopamine‐assisted graphene oxide coating on tetra‐pod zinc oxide whisker for dielectric composites. Chem. Eng. J. 345, 353–363 (2018)
Zuo, Y., et al.: Flexible color‐tunable electroluminescent devices by designing dielectric‐distinguishing double‐stacked emissive layers. Adv. Funct. Mater. 30(50), [eLocator: 2005200] (2020)
Yang, K., et al.: Enhancing dielectric strength of thermally conductive epoxy composites by preventing interfacial charge accumulation using micron‐sized diamond. Compos. Sci. Technol. 221, [eLocator: 109178] (2021)
You have requested "on-the-fly" machine translation of selected content from our databases. This functionality is provided solely for your convenience and is in no way intended to replace human translation. Show full disclaimer
Neither ProQuest nor its licensors make any representations or warranties with respect to the translations. The translations are automatically generated "AS IS" and "AS AVAILABLE" and are not retained in our systems. PROQUEST AND ITS LICENSORS SPECIFICALLY DISCLAIM ANY AND ALL EXPRESS OR IMPLIED WARRANTIES, INCLUDING WITHOUT LIMITATION, ANY WARRANTIES FOR AVAILABILITY, ACCURACY, TIMELINESS, COMPLETENESS, NON-INFRINGMENT, MERCHANTABILITY OR FITNESS FOR A PARTICULAR PURPOSE. Your use of the translations is subject to all use restrictions contained in your Electronic Products License Agreement and by using the translation functionality you agree to forgo any and all claims against ProQuest or its licensors for your use of the translation functionality and any output derived there from. Hide full disclaimer
© 2022. This work is published under http://creativecommons.org/licenses/by-nc-nd/4.0/ (the "License"). Notwithstanding the ProQuest Terms and Conditions, you may use this content in accordance with the terms of the License.
Abstract
Electroluminescent composites have considerable potential for applications in photoelectric display, electric field measurement and other fields due to their advantages of simple preparation and uniform luminescence. However, high voltage required by the operation of electroluminescent composites hinders their applications in the electric domain, and research on the relationship between electroluminescence principle of composites and filler intrinsic attributes is insufficient. In this paper, the effects of electric field strength, filler mass fraction and voltage frequency on the electroluminescence intensity of ZnS:Cu/epoxy composites are studied, which are majorly used as the luminescent layer of electroluminescent devices. To enhance the electroluminescence intensity of composites, high‐temperature sintered BaTiO3 and zinc oxide whiskers (ZnOw) particles are introduced in the base matrix. The finite element method is applied to verify that the matrix of high dielectric constant is in favour of improving the electroluminescence intensity of composites. The band structure of the ZnS:Cu particle is calculated based on the density functional theory + U method to analyse the intrinsic relationship between electroluminescence and particle electronic structure. This paper provides a basis for the research of high electroluminescence intensity devices and will be conducive to better understanding on the relationship between electroluminescence principle and filler intrinsic attributes.
You have requested "on-the-fly" machine translation of selected content from our databases. This functionality is provided solely for your convenience and is in no way intended to replace human translation. Show full disclaimer
Neither ProQuest nor its licensors make any representations or warranties with respect to the translations. The translations are automatically generated "AS IS" and "AS AVAILABLE" and are not retained in our systems. PROQUEST AND ITS LICENSORS SPECIFICALLY DISCLAIM ANY AND ALL EXPRESS OR IMPLIED WARRANTIES, INCLUDING WITHOUT LIMITATION, ANY WARRANTIES FOR AVAILABILITY, ACCURACY, TIMELINESS, COMPLETENESS, NON-INFRINGMENT, MERCHANTABILITY OR FITNESS FOR A PARTICULAR PURPOSE. Your use of the translations is subject to all use restrictions contained in your Electronic Products License Agreement and by using the translation functionality you agree to forgo any and all claims against ProQuest or its licensors for your use of the translation functionality and any output derived there from. Hide full disclaimer
Details



1 State Key Laboratory of Alternate Electrical Power System with Renewable Energy Sources, North China Electric Power University, Beijing, China
2 China Electric Power Research Institute, Beijing, China
3 Electrical Engineering Division, University of Cambridge, Cambridge, UK