1. Introduction
Being the lightest metal structural materials, Mg alloys have shown splendid prospects in the fields of electricity, automobile and aerospace industries. Unfortunately, their relative low strength and poor ductility greatly impeded their further utilization [1,2]. To break through the bottleneck, a series of new Mg-based alloys have been designed and some positive results have been obtained [3,4,5,6,7,8]. Among them, Mg-RE-Zn alloys containing long period stacking ordered (LPSO) phase have received a considerable attention since the discovery of Mg97Y2Zn1 (at.%) alloy, which is produced by rapidly solidified powder metallurgy (RS P/M) technology. The alloy exhibits an excellent yield stress of ~610 MPa, which is about 2.5 times higher than that of conventional Mg alloys. Meanwhile, the elongation of the alloy reaches up to ~5% at room temperature [9]. One of the key factors for such superior mechanical properties is the formation of LPSO phase [9,10,11,12]. So far, a series of LPSO-Mg alloys with superior properties have been developed [13,14,15]. For example, Kawamura et al. [13] prepared an extruded LPSO Mg97Y2Cu1 alloy, which exhibits a yield strength of 297 MPa and an elongation of 8.1% at room temperature. Surperplastic deformation characteristics were also observed in a hot-extruded LPSO Mg-Y-Gd-Zn alloy, which exhibits a maximum elongation of 700% at 470 °C with the strain rate of 1.7 × 10−4 s−1 [14]. In addition, He et al. [15] reported that the high-cycle fatigue strength of an as-cast LPSO Mg-Gd-Zn-Zr alloy can reach 105 MPa, which is much higher than that (20–80 MPa) of the conventional Mg alloys (AZ91, AZ61 and ZE41).
However, most of the investigations in mechanical behaviors of LPSO-Mg alloys were performed under quasi-static loading conditions. In fact, structural materials are inevitably subjected to dynamic loadings in their practical applications, such as impact or collision. Especially for Mg alloys, they often suffer from a sudden failure in these conditions. As is well known, crack propagation is an important process in materials fracture. To the authors’ knowledge, however, the roles of LPSO phase in dynamic crack propagation behavior of LPSO-Mg alloys are still unclear due to the lack of effective experimental methods. In this work, a novel dynamic four-point bent test was performed on an as-cast Mg95.5Y3Zn1.5 alloy, which contains a large volume fraction of LPSO phase. The aim of this work is to reveal the roles of LPSO phase in crack propagation behavior of the alloy under dynamic loadings.
2. Materials and Methods
A Mg95.5Y3Zn1.5 (at.%) ingot was prepared from pure Mg (99.95 wt.%), Zn (99.95 wt.%) and Mg-20Y (wt.%) master alloys in an electric furnace under the protection of a mixed atmosphere of CO2 and SF6 with the ratio of 99:1. The alloy melt was homogenized at 750 °C for 0.5 h, and then poured into a water-cooled mold with a casting temperature of 720 °C. The chemical compositions of the alloy were determined by inductively coupled plasma atomic emission spectroscopy (ICP-AES, Spectro, Kleve, Germany) and the results were listed in Table 1.
The microstructure, phase structure and compositions of the as-cast Mg95.5Y3Zn1.5 alloy were characterized by scanning electron microscopy (SEM, JEOL, Tokyo, Japan) equipped with an X-ray energy dispersive spectrometer (EDS) and transmission electron microscopy (TEM, JEOL, Tokyo, Japan). The thin foil samples for the TEM observation were prepared using the argon ion thinning technique. The volume fraction of the LPSO phase was estimated by image analyzer. Dynamic compression tests were performed on a Split Hopkinson Pressure Bar (SHPB, Harbin Engineering University, Harbin, China) at the strain rates of ~1000 s−1, ~2000 s−1, and ~3000 s−1. The set up of the SHPB is shown in Figure 1a. A pulse shaper was placed at the interface between the striker and the incident bar in order to achieve a constant strain rate and a stress state equilibrium for compression experiments at high strain rates. The incident and the reflected strains were measured by the strain gauges glued at the midpoint of the incident bar, while the transmitted strain was measured by the strain gauges glued at the midpoint of the transmission bar. The dynamic stress, strain and strain rate were calculated using one-dimensional stress wave theory. Specimens used for dynamic compression tests were regular cylinders with an 8 mm diameter and 8 mm height. Each test was repeated eight times to ensure the reliability.
To explicitly observe the crack propagation behavior of the alloy under high strain rate, dynamic four-point bend tests were conducted in this study. The specimens for the tests were double-notched, and the dimensions are shown in Figure 1b. The reason for using such specimens can be explained as follows: as shown in Figure 1c, the cracks initiate at both notches during the dynamic compression process. However, only one crack will propagate to complete rupture, while the other crack generates a certain growth, and then it can be arrested immediately by a sudden unloading. Thus, the evolution information with respect to the fracture process, such as crack paths and their interaction with the second phase, is captured in the non-fractured side of the specimen (especially in the process area as shown in Figure 1c).
3. Results and Discussion 3.1. Microstructure of the As-Cast Mg95.5Y3Zn1.5 Alloy
Figure 2 shows the microstructure of the as-cast Mg95.5Y3Zn1.5 alloy. As shown in Figure 2a, the alloy mainly consists of α-Mg matrix (with dark contrast) and LPSO phase located at the grain boundaries (with grey contrast). The LPSO phase presents lamellar structures with some Mg layers inside the phase, as indicated by the white arrows in Figure 2b. The volume fraction of the LPSO phase is estimated to be ~38% in the as-cast Mg95.5Y3Zn1.5 alloy. Besides, plenty of fine LPSO lamellae are observed in the interior of the Mg matrix, which arrange uniformly with single direction in a whole grain as shown in Figure 2b,c. Figure 2d,e show the EDS results of the as-cast Mg95.5Y3Zn1.5 alloy. The chemical composition of the phase with grey contrast (marked as A in Figure 2c) and the fine lamellar phase (marked as B in Figure 2c) is Mg-6.42 at.% Y-3.76 at.% Zn and Mg-1.26 at.% Y-0.59 at.% Zn, respectively. The composition of the grey phase is equivalent to that of the LPSO phase (Mg-6 at.% Y-4 at.% Zn) observed in the Mg97Y2Zn1 (at.%) alloys [16]. In the case of the lamellar phase, Y and Zn elements are present in a roughly similar proportion of the LPSO phase. In fact, the LPSO phase located at the grain boundaries exhibits a 18R-type LPSO structure, and the LPSO lamellae in Mg matrix exhibit a 14H-type LPSO structure. The confirmation of the LPSO structures was discussed in the following section.
Figure 3a,b show the bright-field (BF) TEM image and the corresponding selected area electron diffraction (SAED) pattern of the LPSO phase, which is located at the grain boundaries, respectively. The SAED pattern shows that the phase exhibits a typical 18R LPSO structure with extra diffractions spots appearing at the ±1/6(0002)α, ±2/6(0002)α…±5/6(0002)α positions [17,18]. In addition, the angle between a* and c* reciprocal vectors is about 83.2° (Figure 3b), which is well consistent with the lattice parameter β = 83.25° of 18R-type LPSO structure [19].
The BF TEM image and the corresponding SAED pattern of the fine LPSO lamellae, which is located within the Mg matrix are shown in Figure 3c,d, respectively. It can be clearly seen that the spots of (00014)14H-LPSO and (0002)α-Mg are coincident in the same position. Moreover, small periodic diffraction spots are found at the interval of 1/14 distance between the transmitted spot and the (0002)α-Mg reflection. The results indicated that the fine lamellae phase within the Mg matrix exhibits a 14H-type LPSO structure [20,21].
3.2. Mechanical Properties of the As-Cast Mg95.5Y3Zn1.5 Alloy
The typical true stress-strain curves of the as-cast Mg95.5Y3Zn1.5 alloy tested under dynamic strain rate (1000 s−1–3000 s−1) loadings are shown in Figure 4. The main mechanical properties are listed in Table 2. The as-cast Mg95.5Y3Zn1.5 alloy exhibits excellent dynamic mechanical properties: for example, the compressive yield stress, the maximum stress and the strain to failure reach up to 190.51 ± 3.52 MPa, 378.32 ± 4.26 MPa and 0.168 ± 0.006, respectively, under the strain rate of ~3000 s−1.
3.3. Crack Propagation Behavior of the As-Cast Mg95.5Y3Zn1.5 Alloy under Dynamic Loadings
Dynamic four-point bend tests were conducted to investigate the role of the LPSO phase in crack propagation behavior of the as-cast Mg95.5Y3Zn1.5 alloy. There were four typical interactions between the cracks and the LPSO phase. Firstly, as shown in Figure 5a, the crack opening displacement (COD) (indicated by the white arrows) increased dramatically form 2.02 μm to 5.52 μm as the crack tip grew to the vicinity of the LPSO phase. Meanwhile, the crack tip became obviously round. This strongly indicates that the crack tip was blunted by the LPSO phase. Secondly, as shown in Figure 5b, the crack entered into the LPSO phase. However, the COD sharply decreased as the crack propagated within the LPSO phase, which indicated that the LPSO phase can effectively impede the crack opening. Previous investigations indicated that LPSO phase itself usually possesses many excellent characteristics, such as high micro-hardness [22] and high toughness [23]. Therefore, the LPSO phase can hinder the entry of the cracks to a large extent. Once the cracks go into the LPSO phase, it can be closed just after a short propagation in the LPSO phase.
Thirdly, due to the strongly hindering effect of LPSO phase on the crack propagation, the propagation direction of the crack is sometimes obviously altered, as shown in Figure 5c. At this point, the crack deflection makes the paths of crack propagation complicated, which enlarges the surface area of crack and increases its propagation distance. Therefore, more energy can be consumed by the additional crack surface area and propagation distance. In addition, the stress state (e.g., the stress value, directions) of the crack tip can be changed after the crack deflection. As a result, the driving force of crack propagation is reduced.
Fourthly, as shown in Figure 5d, the crack consistently propagated along its original direction, but it did not fracture the LPSO phase when it encountered the LPSO phase. The LPSO phase just acted as a “bridge” to connect both sides of the crack surfaces. In this situation, the LPSO phase is expected to offer a closure stress, which makes the crack surfaces close to each other. Hence, the crack opening is hindered by the LPSO phase. It is considered that the LPSO phase can toughen the alloy via a “crack bridging” mechanism.
Based on above analysis, the LPSO phase indeed plays a key role in hindering the crack propagation under high strain rate loading, which results in the improvement of the dynamic mechanical properties. On one hand, to overcome the hindering of LPSO phase, the crack propagation needs larger stress. That is to say, the hindering effects of LPSO phase on crack propagation enhance the strength of the alloy. On the other hand, those effects also prevent the alloy from premature fracture and lead to a high ductility.
4. Conclusions
In this work, the crack propagation behavior of an as-cast Mg95.5Y3Zn1.5 alloy was investigated under dynamic strain rate loadings. The main results can be summarized as follows: (1)
The as-cast Mg95.5Y3Zn1.5 alloy mainly consists of α-Mg matrix, 18R LPSO phase located at the grain boundaries and 14H LPSO lamellae located within the Mg matrix. (2)
The as-cast Mg95.5Y3Zn1.5 alloy exhibits excellent dynamic mechanical properties: the compressive yield stress, maximum stress and strain to failure are 190.51 ± 3.52 MPa, 378.32 ± 4.26 MPa and 0.168 ± 0.006, respectively, at the strain rate of ~3000 s−1. (3)
The LPSO phase plays an important role in hindering dynamic crack propagation, through crack tip blunting, crack opening inhibition, crack deflection and crack bridging.
Figure 1.(a) Illustration of the Split Hopkinson Pressure Bar; (b) Dimensions of the specimens used in dynamic four-point bend tests; (c) Mechanism of the dynamic four-point bend tests used in this study.
Figure 2.(a-c) microstructures of the as-cast Mg95.5Y3Zn1.5 alloy; (d) energy dispersive spectrometer (EDS) results of the point A in (c); (e) EDS results of the point B in (c).
Figure 3. Transmission electron microscopy (TEM) bright field images and selected area electron diffraction (SAED) patterns of the long period stacking ordered (LPSO) phases in the as-cast Mg95.5Y3Zn1.5 alloy: (a,b) LPSO phase located at the grain boundaries; (c,d) LPSO lamellae located within the Mg matrix.
Figure 4. True stress-strain curves of the as-cast Mg95.5Y3Zn1.5 alloy tested at the strain rates of ~1000 s-1, ~2000 s-1, and ~3000 s-1.
Figure 5. Microstructure of the as-cast Mg95.5Y3Zn1.5 alloy after dynamic deformation at the strain rate of ~3000 s-1, showing the relationships between the cracks and LPSO phase: (a) Crack tip blunting (the white arrows indicated crack opening displacement); (b) Crack opening inhibition; (c) Crack deflection; (d) Crack bridging.
Alloy | Chemical Compositions (at.%) | |||||
---|---|---|---|---|---|---|
Y | Zn | Fe | Ni | Cu | Mg | |
Mg95.5Y3Zn1.5 | 3.4201 | 1.6328 | 0.0026 | 0.0015 | 0.0010 | Bal. |
Alloy | Yield Stress (MPa) | Maximum Stress (MPa) | Strain to Failure (%) | Strain Rate (s−1) |
---|---|---|---|---|
Mg95.5Y3Zn1.5 | 181.62 ± 3.28 | 365.56 ± 5.16 | 0.182 ± 0.008 | ~1000 |
186.45 ± 2.90 | 372.65 ± 4.80 | 0.176 ± 0.006 | ~2000 | |
190.51 ± 3.52 | 378.32 ± 4.26 | 0.168 ± 0.006 | ~3000 |
Author Contributions
Literature search: X.S., Y.L., H.Z., L.C. and Y.Z.; data collection and analysis: X.S., Y.L., L.C., Y.Z., X.Y. (Xiaoming Yu), X.Y. (Xuan Yu) and L.C.; writing original draft: X.S., Y.L., H.Z., L.C., Y.Z., X.Y. (Xiaoming Yu), X.Y. (Xuan Yu), L.C. and Z.L.; revising and editing: L.C. and Z.L.
Funding
This research was funded by Natural Science Foundation of Zhejiang Province, grant number LY19E010005; National Natural Science Foundation of China, grant number 51501046 and Zhoushan Science and Technology Project, grant number 2018C21025.
Conflicts of Interest
The authors declare no conflict of interest.
© 2019 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license (http://creativecommons.org/licenses/by/4.0/).
1. Joost, W.J.; Krajewski, P.E. Towards magnesium alloys for high-volume automotive applications. Scr. Mater. 2017, 128, 107-112.
2. Wu, X.; Pan, F.; Cheng, R.; Luo, S. Effect of morphology of long period stacking ordered phase on mechanical properties of Mg-10Gd-1Zn-0.5 Zr magnesium alloy. Mater. Sci. Eng. A 2018, 726, 64-68.
3. You, S.; Huang, Y.; Ulrich, K.; Hort, N. Recent research and developments on wrought magnesium alloys. J. Magnes. Alloys 2017, 5, 239-253.
4. Sabat, R.K.; Brahme, A.P.; Mishra, R.K.; Inal, K.; Suwas, S. Ductility enhancement in Mg-0.2%Ce alloys. Acta Mater. 2018, 161, 246-257.
5. Alaneme, K.K.; Okotete, E.A. Enhancing plastic deformability of Mg and its alloys-A review of traditional and nascent developments. J. Magnes. Alloys 2017, 4, 460-475.
6. Kang, Q.; Jiang, H.; Zhang, Y.; Xu, Z.; Li, H.; Xia, Z. Effect of various Ca content on microstructure and fracture toughness of extruded Mg-2Zn alloys. J. Alloys Compds 2018, 742, 1019-1030.
7. Nie, J.F. Precipitation and hardening in magnesium alloys. Metall. Mater. Trans. A 2012, 43A, 3891-3939.
8. Li, Y.; Yang, C.; Zeng, X.; Jin, P.; Qiu, D.; Ding, W. Microstructure evolution and mechanical properties of magnesium alloys containing long period stacking ordered phase. Mater. Charact. 2018, 141, 286-295.
9. Kawamura, Y.; Hayashi, K.; Inoue, A.; Masumoyo, T. Rapidly solidified powder metallurgy Mg97Zn1Y2 alloys with excellent tensile yield strength above 600 MPa. Mater. Trans. 2001, 42, 1171-1174.
10. Xu, D.K.; Han, E.H.; Xu, Y.B. Effect of long-period stacking ordered phase on microstructure, mechanical property and corrosion resistance of Mg alloys: A review. Prog. Nat. Sci. Mater. 2016, 26, 117-128. [Green Version]
11. Chen, R.; Sandlöbes, S.; Zehnder, C.; Zeng, X. Deformation mechanisms, activated slip systems and critical resolved shear stresses in an Mg-LPSO alloy studied by micro-pillar compression. Mater. Des. 2018, 154, 203-216.
12. Lü, S.; Wu, S.; Yang, X.; Hao, L.; Guo, W.; Fang, X. Microstructure and mechanical properties of Mg97Zn1Y2 alloy reinforced with LPSO structure produced by semisolid squeeze casting. Mater. Sci. Eng. A 2018, 732, 359-367.
13. Kawamura, Y.; Kasahara, T.; Izumi, S.; Yamasaki, M. Elevated temperature Mg97Y2Cu1 alloy with long period ordered structure. Scr. Mater. 2006, 55, 453-456.
14. Zhang, L.; Zhang, J.; Xu, C.; Liu, S.; Jiao, Y.; Xu, L.; Wang, Y. Investigation of high-strength and superplastic Mg-Y-Gd-Zn alloy. Mater. Des. 2014, 61, 168-176.
15. He, Z.; Fu, P.; Wu, Y. High cycle fatigue behavior of as-cast Mg96.34Gd2.5Zn1Zr0.16 alloy fabricated by semi-continuous casting. Mater. Sci. Eng. A 2013, 587, 72-78.
16. Itoi, T.; Seimiya, T.; Kawamura, Y. Long period stacking structures observed in Mg97Zn1Y2 alloy. Scr. Mater. 2004, 51, 107-111.
17. Xu, C.; Xu, S.W.; Zheng, M.Y. Microstructures and mechanical properties of high-strength Mg-Gd-Y-Zn-Zr alloy sheets processed by severe hot rolling. J. Alloys Compds 2012, 524, 46-52.
18. Egusa, D.; Abe, E. The structure of long period stacking/order Mg-Zn-RE phases with extended non-stoichiometry ranges. Acta Mater. 2012, 60, 166-178.
19. Zhu, Y.M.; Morton, A.J.; Nie, J.F. The 18R and 14H long-period stacking ordered structures in Mg-Y-Zn alloys. Acta Mater. 2010, 58, 2936-2947.
20. Zou, G.; Cai, X.; Fang, D. Age strengthening behavior and mechanical properties of Mg-Dy based alloys containing LPSO phases. Mater. Sci. Eng. A 2015, 620, 10-15.
21. Zhang, J.; Chen, C.; Que, Z. 18R and 14H long-period stacking ordered structures in the Mg93.96Zn2Y4Sr0.04 alloy and the modification effect of Sr on X-phase. Mater. Sci. Eng. A 2012, 552, 81-88.
22. Li, D.; Zhang, J.; Que, Z. Effects of Mn on the microstructure and mechanical properties of long period stacking ordered Mg95Zn2.5Y2.5 alloy. Mater. Lett. 2013, 109, 46-50.
23. Leng, Z.; Zhang, J.; Yin, T. Microstructure and mechanical properties of Mg-9RY-4Cu alloy with long period stacking ordered phase. Mater. Sci. Eng. A 2013, 580, 196-201.
Innovation and Application Institute, Zhejiang Ocean University, Zhoushan 316022, China
*Author to whom correspondence should be addressed.
You have requested "on-the-fly" machine translation of selected content from our databases. This functionality is provided solely for your convenience and is in no way intended to replace human translation. Show full disclaimer
Neither ProQuest nor its licensors make any representations or warranties with respect to the translations. The translations are automatically generated "AS IS" and "AS AVAILABLE" and are not retained in our systems. PROQUEST AND ITS LICENSORS SPECIFICALLY DISCLAIM ANY AND ALL EXPRESS OR IMPLIED WARRANTIES, INCLUDING WITHOUT LIMITATION, ANY WARRANTIES FOR AVAILABILITY, ACCURACY, TIMELINESS, COMPLETENESS, NON-INFRINGMENT, MERCHANTABILITY OR FITNESS FOR A PARTICULAR PURPOSE. Your use of the translations is subject to all use restrictions contained in your Electronic Products License Agreement and by using the translation functionality you agree to forgo any and all claims against ProQuest or its licensors for your use of the translation functionality and any output derived there from. Hide full disclaimer
© 2019. This work is licensed under https://creativecommons.org/licenses/by/4.0/ (the “License”). Notwithstanding the ProQuest Terms and Conditions, you may use this content in accordance with the terms of the License.
Abstract
[...]structural materials are inevitably subjected to dynamic loadings in their practical applications, such as impact or collision. [...]only one crack will propagate to complete rupture, while the other crack generates a certain growth, and then it can be arrested immediately by a sudden unloading. [...]the evolution information with respect to the fracture process, such as crack paths and their interaction with the second phase, is captured in the non-fractured side of the specimen (especially in the process area as shown in Figure 1c). [...]the LPSO phase located at the grain boundaries exhibits a 18R-type LPSO structure, and the LPSO lamellae in Mg matrix exhibit a 14H-type LPSO structure. [...]small periodic diffraction spots are found at the interval of 1/14 distance between the transmitted spot and the (0002)α-Mg reflection.
You have requested "on-the-fly" machine translation of selected content from our databases. This functionality is provided solely for your convenience and is in no way intended to replace human translation. Show full disclaimer
Neither ProQuest nor its licensors make any representations or warranties with respect to the translations. The translations are automatically generated "AS IS" and "AS AVAILABLE" and are not retained in our systems. PROQUEST AND ITS LICENSORS SPECIFICALLY DISCLAIM ANY AND ALL EXPRESS OR IMPLIED WARRANTIES, INCLUDING WITHOUT LIMITATION, ANY WARRANTIES FOR AVAILABILITY, ACCURACY, TIMELINESS, COMPLETENESS, NON-INFRINGMENT, MERCHANTABILITY OR FITNESS FOR A PARTICULAR PURPOSE. Your use of the translations is subject to all use restrictions contained in your Electronic Products License Agreement and by using the translation functionality you agree to forgo any and all claims against ProQuest or its licensors for your use of the translation functionality and any output derived there from. Hide full disclaimer